Preparation method and application of semiconductor sulfide composite nanofiber membrane
The transition metal sulfide is combined with a high-molecular polymer through electrospinning to prepare a semiconductor sulfide composite nanofiber membrane, which solves the problems of low precision in traditional material detection and material morphology that hinders its application, and achieves efficient detection of heavy metal cations. And suitable for large-scale production.
Patent Information
- Application Number
- CN202410013992.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-04
AI Technical Summary
Traditional polymer ion exchange materials have high ion rejection rates in ion detection, resulting in low detection precision, and the transition metal sulfide powder form hinders their application in heavy metal cation detection.
The electrospinning method is used to combine transition metal sulfides with high molecular polymers to prepare semiconductor sulfide composite nanofiber membranes. The nanofibers are pretreated and activated to improve their responsiveness to metal ions.
The ion rejection rate of the polymer membrane is reduced, the capture ability of heavy metal cations is improved, and the detection sensitivity is enhanced. The preparation method is simple and low-cost, and is suitable for large-scale production.
Smart Images

Figure CN117867761B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material preparation, and particularly relates to a preparation method and application of a semiconductor sulfide composite nanofiber membrane. Background Art
[0002] Ion retention rate refers to the ability of ions in a solution to be fixed on a solid surface during the ion exchange process. In the process of water treatment using membrane materials, changes in ion retention rate show the ability of the film to regulate the speed at which heavy metal cations in water are conducted into the membrane material. However, the large family of polymer exchange membrane materials currently developed focuses more on improving ion retention rate and is applied to solution ion separation. In the field of precision detection, low ion retention rate and faster ion conduction ability can collect the ions to be measured, thereby improving the detection precision of the ions to be measured. Therefore, there is an urgent need for effective methods to change the retention rate properties of traditional polymer exchange materials and realize effective applications in ion detection sensors.
[0003] Traditional polymer ion exchange materials mostly exist as insulating properties. At present, in ion detection applications, based on the requirements of the detection platform, one of the important conditions is that the material has good conductivity. Therefore, it is urgent and important to study how to change the properties of traditional polymer materials and realize the application of solution cation detection.
[0004] Transition metal sulfides have unique ion adsorption, low price, and certain ion conductivity, making them potential detection materials in the future. Compared with high molecular polymers, they have higher electrical conductivity. Although transition metal sulfides have unique ion conductivity for heavy metal cations, their powder form seriously hinders their practical application. There is no method for combining transition metal sulfides with high molecular polymers for heavy metal cation detection. At the same time, the modification of powder form is one of the hot topics in the detection and energy fields. Summary of the invention
[0005] In view of the problems existing in the above-mentioned prior art, the object of the present invention is to provide a preparation method and application of a semiconductor sulfide composite nanofiber membrane.
[0006] In order to achieve the above technical objectives, the present invention provides the following technical solutions:
[0007] A first aspect of the present invention provides a method for preparing a semiconductor sulfide composite nanofiber membrane, comprising the following steps:
[0008] S1. Using a first alkaline solution to stir, wash and dry the transition metal sulfide powder to obtain a pretreated powder;
[0009] S2, adding the obtained pretreated powder and high molecular polymer into a solvent, stirring and mixing evenly to obtain a mixed spinning solution;
[0010] S3, loading the obtained mixed spinning solution into an electrospinning device, performing electrospinning, and drying to obtain a transition metal sulfide composite nanofiber prefabricated membrane;
[0011] S4, immersing the obtained transition metal sulfide composite nanofiber prefabricated membrane into a second alkaline solution, washing and drying, to obtain a semiconductor sulfide composite nanofiber membrane.
[0012] Preferably, the transition metal sulfide powder is one of zinc sulfide, cadmium sulfide, zinc cadmium sulfide, or a combination of two or more thereof.
[0013] Preferably, in step S1, the first alkaline solution is one or a combination of two or more of ammonia water, sodium hydroxide, potassium hydroxide, ammonium hydroxide, sodium sulfide, sodium sulfite, sodium carbonate, and sodium bicarbonate.
[0014] Preferably, in step S1, the stirring and washing time is 6 to 48 hours.
[0015] Preferably, in step S2, the high molecular polymer is one or a combination of two or more of polyacrylonitrile, polyvinylidene fluoride, polyimide, polyamic acid, polystyrene and polylactic acid.
[0016] Preferably, in step S2, the mass ratio of the transition metal sulfide powder to the high molecular polymer is 1:70:100.
[0017] Preferably, in step S2, the stirring and mixing temperature is 40-80° C., and the stirring time is 2-24 hours.
[0018] Preferably, in step S3, the conditions for electrospinning are: the injection speed of the mixed solution is 0.01 2 mL / h, and the potential difference is 10 50 V.
[0019] Preferably, in step S4, the second alkaline solution is one or a combination of two or more of ammonia water, sodium hydroxide, potassium hydroxide, ammonium hydroxide, sodium sulfide, sodium sulfite, sodium carbonate, and sodium bicarbonate.
[0020] The second aspect of the present invention provides a semiconductor sulfide composite nanofiber membrane obtained by the above preparation method. The semiconductor sulfide composite nanofiber membrane is a thin film with adjustable thickness, length and width, and a nanofiber microstructure. The nanofibers are composed of a semiconductor sulfide and a high molecular polymer composite material, and the outer layer of the fiber is a high molecular polymer.
[0021] The third aspect of the present invention provides the use of the semiconductor sulfide composite nanofiber membrane (as an adsorption layer) in a sensor for detecting heavy metal ion concentration.
[0022] The present invention has the following beneficial effects:
[0023] (1) The present invention uses transition metal sulfide and high molecular polymer as raw materials and adopts electrospinning to synthesize semiconductor sulfide composite nanofiber membrane. By introducing semiconductor transition metal sulfide, the ion retention rate of the high molecular polymer membrane can be reduced, making it easier to capture more heavy metal cations, and more sensitive when used as an adsorption layer for sensor detection.
[0024] (2) In the present invention, pre-treating the transition metal sulfide with a first alkaline solution can increase the interface bonding between the transition metal sulfide and the polymer material, and pre-treating the prefabricated nanofiber membrane with a second alkaline solution to activate the nanofibers can make them more sensitive to metal ions.
[0025] (3) The present invention adopts electrospinning to synthesize semiconductor sulfide composite nanofiber membranes with expandable length, width and thickness. The experimental results show that the zinc cadmium sulfide (Zn x Cd 1-x S) Composite nanofiber membrane, due to its unique structure and composition, has high reactivity and can be used as a sensor.
[0026] (4) The preparation method of the present invention is scientific, simple, reasonable, easy to implement, and low-cost, and is suitable for large-scale production of large-scale films. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 This is an optical picture of the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1;
[0029] Figure 2 This is a SEM image of the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1;
[0030] Figure 3 This is a TEM analysis diagram of the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1;
[0031] Figure 4The contact angle images of the semiconductor zinc cadmium sulfide composite nanofiber membrane, the pure polymer membrane and the composite membrane not treated with alkaline solution prepared in Example 1;
[0032] Figure 5 Zeta potential results of the semiconductor zinc cadmium sulfide composite nanofiber membrane, pure polymer membrane and composite membrane not treated with alkaline solution prepared in Example 1;
[0033] Figure 6 These are the EIS electrochemical test results of the semiconductor zinc cadmium sulfide composite nanofiber membrane, pure polymer membrane, and composite membrane not treated with alkaline solution prepared in Example 1. DETAILED DESCRIPTION
[0034] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present invention.
[0035] Example 1
[0036] 60 mg of zinc cadmium sulfide powder and sodium hydroxide were weighed and placed in a beaker, and stirred at a speed of 500 r / min for 12 h. The mixed solution was filtered, and the washed product was dried in a vacuum drying oven at 80 ° C for 24 h to obtain pretreated zinc sulfide powder; the prepared pretreated zinc cadmium sulfide powder and 2 g of polyacrylonitrile powder were placed in a beaker, 25 mL of N, N-dimethylformamide was added, and stirred at 60 ° C for 12 h to obtain a uniformly distributed mixed solution; the mixed solution was transferred to an electrospinning device and heated at 0.3 mL·h -1 The mixed solution was electrospun at an injection flow rate of 20V and a potential difference of 20V to obtain a zinc cadmium sulfide composite nanofiber prefilm, and then the obtained prefilm was immersed in sodium hydroxide, washed and dried to obtain a semiconductor zinc cadmium sulfide composite nanofiber membrane.
[0037] Example 2
[0038] 60 mg of zinc sulfide powder and sodium hydroxide were weighed and placed in a beaker, and stirred at a speed of 500 r / min for 12 h. The mixed solution was filtered, and the washed product was dried in a vacuum drying oven at 80 ° C for 24 h to obtain pretreated zinc sulfide powder; the prepared pretreated zinc sulfide powder and 2 g of polyacrylonitrile powder were placed in a beaker, 25 mL of N, N-dimethylformamide was added, and stirred at 60 ° C for 12 h to obtain a uniformly distributed mixed solution; the mixed solution was transferred to an electrospinning device and heated at 0.3 mL·h -1The mixed solution was electrospun at an injection flow rate of 30V and a potential difference of 30V to obtain a zinc sulfide composite nanofiber prefilm, and then the obtained prefilm was immersed in sodium hydroxide, washed and dried to obtain a semiconductor zinc sulfide composite nanofiber membrane.
[0039] Example 3
[0040] 40 mg of zinc sulfide powder and potassium hydroxide were weighed and placed in a beaker, and stirred at a speed of 500 r / min for 6 h. The mixed solution was filtered, and the washed product was dried in a vacuum drying oven at 60 ° C for 12 h to obtain pretreated zinc sulfide powder; the prepared pretreated zinc sulfide powder and 2 g of polyacrylonitrile powder were placed in a beaker, 25 mL of N, N-dimethylformamide was added, and stirred at 60 ° C for 12 h to obtain a uniformly distributed mixed solution; the mixed solution was transferred to an electrospinning device and heated at 0.6 mL·h -1 The mixed solution was electrospun at an injection flow rate of 50V and a potential difference of 50V to obtain a zinc sulfide composite nanofiber prefilm, and then the obtained prefilm was immersed in potassium hydroxide, washed and dried to obtain a semiconductor zinc sulfide composite nanofiber membrane.
[0041] Example 4
[0042] 10 mg of cadmium sulfide powder and sodium hydroxide were weighed and placed in a beaker, and stirred at a speed of 500 r / min for 24 h. The mixed solution was filtered, and the washed product was dried in a vacuum drying oven at 50 ° C for 10 h to obtain a pretreated cadmium sulfide powder; the prepared pretreated cadmium sulfide powder and 100 mg of polyacrylonitrile powder were placed in a beaker, 25 mL of N, N-dimethylformamide was added, and stirred at 60 ° C for 12 h to obtain a uniformly distributed mixed solution; the mixed solution was transferred to an electrospinning device and heated at 0.6 mL·h -1 The mixed solution was electrospun at an injection flow rate of 10 V and a potential difference of 10 V to obtain a cadmium sulfide composite nanofiber prefilm, and then the obtained prefilm was immersed in sodium carbonate, washed and dried to obtain a semiconductor cadmium sulfide composite nanofiber membrane.
[0043] Comparative Example 1
[0044] The polyacrylonitrile film was used as a control and recorded as pure polymer film.
[0045] Comparative Example 2
[0046] The steps are basically the same as those in Example 1, except that the zinc cadmium sulfide powder is not pretreated with sodium hydroxide, and the prefabricated nanofiber membrane is not pretreated with sodium hydroxide to obtain a composite membrane that is not treated with an alkaline solution.
[0047] The appearance structure of the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1 was analyzed. Figure 1 .
[0048] Depend on Figure 1 The results show that the prepared semiconductor zinc cadmium sulfide composite nanofiber membrane is a thin film with an expandable length of 32 cm in length and 16 cm in width.
[0049] The morphology and structure of the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1 were analyzed, and the SEM results are shown in Figure 2 .Depend on Figure 2 The results show that in the prepared semiconductor zinc cadmium sulfide composite nanofiber membrane, all fibers are nanofiber size.
[0050] TEM analysis was performed on the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1, the pure polymer membrane in Comparative Example 1, and the composite membrane prepared in Comparative Example 2 without alkaline solution treatment. The results are shown in FIG. Figure 3 .Depend on Figure 3 It can be observed from the results that in the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1, the semiconductor zinc cadmium sulfide is completely embedded in the polyacrylonitrile.
[0051] Test Example 1
[0052] The semiconductor zinc cadmium sulfide composite nanofiber membrane prepared in Example 1 (referred to as the alkaline solution treated composite membrane), the pure polymer membrane in Comparative Example 1, and the composite membrane prepared in Comparative Example 2 without alkaline solution treatment were cut into circular films with a radius of 1 cm. 30 mL of 10 mg / L Cr 6+ The solution was dripped onto the above film and allowed to stand for 5 minutes. The film was placed in an ion electrokinetic test cell for electrochemical impedance spectroscopy to obtain the impedance data of the film and analyze the ability of the composite nanofiber membrane prepared in this embodiment to conduct heavy metal ion liquid. Figure 4 and Figure 5 .
[0053] Depend on Figure 4 and Figure 5 The results show that compared with the pure polymer membrane and the composite membrane not treated with alkaline solution, the semiconductor zinc cadmium sulfide composite nanofiber membrane sample prepared by the present invention has a faster conduction 6+ The ability of the solution indicates that the semiconductor zinc cadmium sulfide composite nanofiber membrane has a stronger ability to adsorb Cr 6+ ability.
[0054] The above adsorption of Cr 6+ The sensing ability of the semiconductor zinc cadmium sulfide composite nanofiber membrane (referred to as the alkaline solution treated composite membrane), the pure polymer membrane and the composite membrane not treated with alkaline solution were tested. The results are shown in Figure 6 .Depend on Figure 6The results show that compared with the polymer membrane and the composite membrane not treated with alkaline solution, the semiconductor zinc cadmium sulfide composite nanofiber membrane prepared by the present invention shows good resistance to Cr 6+ In summary, the zinc cadmium sulfide (Zn x Cd 1-x S) Composite nanofiber membrane, due to its unique structure and composition, has high reactivity and can be used as a sensor.
[0055] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.
Claims
1. A method for preparing a semiconductor sulfide composite nanofiber membrane, characterized in that: The following steps are involved: S1. Using a first alkaline solution, stirring, washing, and drying the transition metal sulfide powder to obtain a pretreated powder; S2, adding the obtained pretreated powder and high molecular weight polymer into a solvent, stirring and mixing them uniformly to obtain a mixed spinning solution; S3, loading the obtained mixed spinning solution into an electrospinning device, performing electrospinning, and drying to obtain a sulfide composite nanofiber prefabricated membrane; The electrospinning conditions are as follows: the injection rate of the mixed solution is 0.01-2 mL / h, the potential difference is 10-50 V; S4, immersing the obtained sulfide composite nanofiber prefabricated membrane in a second alkaline solution, washing and drying, to obtain a semiconductor sulfide composite nanofiber membrane; The high molecular polymer is one or a combination of two or more of polyacrylonitrile, polyvinylidene fluoride, polyimide, polyamic acid, polystyrene and polylactic acid; Pretreating the transition metal sulfide powder with a first alkaline solution can increase the interface bonding between the transition metal sulfide powder and the polymer material, and pretreating the sulfide composite nanofiber prefabricated membrane with a second alkaline solution to activate the nanofibers can make them more sensitive to metal ions.
2. The method for preparing a semiconductor sulfide composite nanofiber membrane according to claim 1, characterized in that: The transition metal sulfide powder is one of zinc sulfide, cadmium sulfide, and zinc cadmium sulfide, or a combination of two or more thereof; the first alkaline solution is one of ammonia water, sodium hydroxide, potassium hydroxide, ammonium hydroxide, sodium sulfide, sodium sulfite, sodium carbonate, and sodium bicarbonate, or a combination of two or more thereof.
3. The method for preparing the semiconductor sulfide composite nanofiber membrane according to claim 1, characterized in that: In step S1, the stirring and washing time is 6 to 48 hours.
4. The method for preparing a semiconductor sulfide composite nanofiber membrane according to claim 1, characterized in that: In step S2, the mass ratio of the transition metal sulfide powder to the high molecular weight polymer is 1-70:
100.
5. The method for preparing a semiconductor sulfide composite nanofiber membrane according to claim 1, characterized in that: In step S2, the stirring and mixing temperature is 40-80° C., and the stirring time is 2-24 hours.
6. The method for preparing a semiconductor sulfide composite nanofiber membrane according to claim 1, characterized in that: In step S4, the second alkaline solution is one or a combination of two or more of ammonia water, sodium hydroxide, potassium hydroxide, ammonium hydroxide, sodium sulfide, sodium sulfite, sodium carbonate, and sodium bicarbonate.
7. A semiconductor sulfide composite nanofiber membrane prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the semiconductor sulfide composite nanofiber membrane according to claim 7 in a sensor for detecting heavy metal ion concentration.
Citation Information
Patent Citations
Nano zine sulfide, solution preparation and method and device for film forming on metal or compound surface
CN101012554A
Preparation method and use of carboxyl-modified polyacrylonitrile nano fiber membrane
CN102389724A
Self-assembly electrostatic spinning nanofiber membrane for absorbing heavy metal ions and preparation method of self-assembly electrostatic spinning nanofiber membrane
CN103212382A
Method for preparing cadmium sulfide nanopowder
CN103214027A
Electrostatic spinning nanofiber membrane as well as preparation method thereof
CN103437071A