Solid electrolyte material, composite solid electrolyte and preparation method thereof, and solid-state lithium battery

Through the treatment of multi-element collaborative doping and specific D50 control, the problem of poor crystal structure stability of LLZO solid electrolyte materials is solved, high ionic conductivity and long cycle time are achieved, and the stability and safety in water are enhanced. Industrialized production.

CN117878386BActive Publication Date: 2024-11-29BEIJING EASPRING MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311623390.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-11-29
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

The crystal structure stability of existing LLZO solid electrolyte materials is poor, especially instability in water, which leads to safety hazards of lithium batteries in high or low temperature environments.

Method used

Through multi-element co-doping and specific D50-controlled mixing treatment, O-Zr-O bond length and bond angle are regulated, the crystal structure stability of solid electrolyte materials is improved, and wet grinding and low-temperature sintering technology are used to reduce the synthesis temperature. , enhance stability in water.

Benefits of technology

It realizes high ionic conductivity and long cycle time of solid electrolyte materials, improves stability and safety in water, reduces safety risks and costs in nanoification, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117878386B_ABST
    Figure CN117878386B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of lithium batteries, and discloses a solid electrolyte material, a composite solid electrolyte, a preparation method thereof, and a solid lithium battery. The crystal structure of the solid electrolyte material satisfies: the O-Zr-O bond length is or the O-Zr-O bond angle is 176.30°-179.97° or 180.03°-183.70°. The crystal structure of the solid electrolyte material has good stability, is stable to air and water, and is especially stable in water; in addition, the solid electrolyte material has high ionic conductivity and long cycle time. The method has a simple production process, is easy to operate, and is very suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium batteries, and in particular to solid electrolyte materials, composite solid electrolytes, preparation methods thereof, and solid lithium batteries. Background Art

[0002] Liquid lithium-ion batteries have safety risks, and the main cause is the liquid electrolyte. The main cause of electric vehicle safety accidents is thermal runaway, which leads to battery explosion or spontaneous combustion. The cause of battery spontaneous combustion is that the power battery short-circuits under overcharge, low temperature or high temperature environment, and the battery releases a lot of heat in a short period of time, igniting the liquid electrolyte inside the battery, and eventually causing the battery to catch fire.

[0003] Cubic phase lanthanum lithium zirconate Li7La3Zr2O 12 (LLZO) solid electrolyte material has a high ion transfer number (t Li ≈1), high ionic conductivity ((σ Li ≈10 -4 -10 -3 S / cm), wide electrochemical window (0-6V vs Li + / Li), is stable to lithium metal, and has good manufacturing processability. Cubic phase nano LLZO has good application prospects in composite electrolytes, coated diaphragms, positive electrode modification, and lithium metal negative electrode modification. The solid phase method often requires a higher sintering temperature (>1000℃) in the preparation of cubic phase LLZO, which increases the difficulty of nano-sizing.

[0004] CN109935901A discloses a Nb and Ta co-doped garnet-type LLZO solid electrolyte and a preparation method thereof. In the process of synthesizing the LLZO electrolyte material, the lanthanum source needs to be pre-sintered to remove moisture, which will reduce the sintering activity of lanthanum oxide, and further, it is necessary to use isopropanol as a medium for wet ball milling to reduce the difficulty of sintering.

[0005] Therefore, it is of great significance to design and develop low-temperature synthesized cubic phase LLZO solid electrolyte materials and their preparation methods. Summary of the invention

[0006] The purpose of the present invention is to overcome the problem of poor crystal structure stability of LLZO solid electrolyte materials in the prior art.

[0007] In order to achieve the above object, the first aspect of the present invention provides a solid electrolyte material, the crystal structure of the solid electrolyte material satisfies: the O-Zr-O bond length is or The O-Zr-O bond angle is 176.30°-179.97° or 180.03°-183.70°.

[0008] A second aspect of the present invention provides a method for preparing the solid electrolyte material according to the first aspect, the method comprising the following steps:

[0009] (1) In the presence of a solvent, a lithium source, a lanthanum source, a zirconium source, a phosphorus source and M 1 The source is mixed and ground, and the obtained product is dried to obtain a mixed material; wherein the mixed material also contains M 2 Source and / or M 3 Source: D of the mixture 50 <0.5μm, D 100 <1μm;

[0010] (2) In a dry atmosphere, the mixed material is sequentially sintered, crushed, sieved and iron-removed.

[0011] A third aspect of the present invention provides a composite solid electrolyte, which comprises the solid electrolyte material described in the first aspect, a lithium salt and a binder.

[0012] A fourth aspect of the present invention provides a method for preparing the composite solid electrolyte according to the third aspect, the preparation method comprising:

[0013] (1) mixing a solid electrolyte material, a lithium salt and a binder to obtain a mixed product;

[0014] (2) subjecting the kneaded product to hot pressing.

[0015] A fifth aspect of the present invention provides a solid-state lithium battery, comprising a positive electrode, an electrolyte and a negative electrode, wherein the electrolyte is the composite solid-state electrolyte described in the third aspect.

[0016] Through the above technical solution, the present invention has the following advantages:

[0017] (1) The crystal structure of the solid electrolyte material provided by the present invention satisfies: the O-Zr-O bond length is or The O-Zr-O bond angle is 176.30°-179.97° or 180.03°-183.70°. The solid electrolyte material has good crystal structure stability, is stable to air and water, and is especially stable in water; in addition, the solid electrolyte material has high ion conductivity and long cycle time;

[0018] (2) The method provided by the present invention is to coordinate the doping of multiple elements to prepare the specific D 50Control can effectively regulate the O-Zr-O bond length and O-Zr-O bond angle of the solid electrolyte material to improve its crystal structure stability, especially stability in water. In a preferred case, the method provided by the present invention can effectively reduce the synthesis temperature of the cubic garnet solid electrolyte material, and the hollow structure particles are easy to nano-scale; in the process of nano-scale, water can also be used as a solvent, which can effectively reduce the safety issues in the process of nano-scale using organic solvents, and the cost is lower; in addition, the method has a simple production process, is easy to operate, and is very suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is the X-ray diffraction pattern of the solid electrolyte material prepared in Example 1 and Comparative Example 1 of the present invention and the cubic phase LLZO standard card PDF#01-090-2617;

[0020] Figure 2 is a scanning electron microscope image of the solid electrolyte material prepared in Example 1 of the present invention;

[0021] Figure 3 is a cross-sectional view of a solid electrolyte material prepared in Example 1 of the present invention;

[0022] Figure 4 is a cross-sectional view of a solid electrolyte material prepared in Example 1 of the present invention;

[0023] Figure 5 is a scanning electron microscope image of the solid electrolyte material prepared in Comparative Example 1;

[0024] Figure 6 is a cross-sectional view of the solid electrolyte material prepared in Comparative Example 1;

[0025] Figure 7 It is the X-ray diffraction pattern of the solid electrolyte material prepared in Example 1, Example 10 and Comparative Examples 2-3 of the present invention after ball milling in water for 300 minutes and drying. DETAILED DESCRIPTION

[0026] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0027] In the present invention, unless otherwise specified, "first" and "second" do not represent a sequence of precedence or a limitation on each material or operation. They are only used to distinguish each material or operation. For example, the "first" and "second" in "first stage" and "second stage" are only used to distinguish and indicate that these are not the same sintering stages.

[0028] As mentioned above, the first aspect of the present invention provides a cubic garnet-type solid electrolyte material, the crystal structure of which satisfies: the O-Zr-O bond length is or The O-Zr-O bond angle is 176.30°-179.97° or 180.03°-183.70°.

[0029] The inventors of the present invention discovered during the research process that the solid electrolyte material satisfying the above-mentioned specific crystal structure has good crystal structure stability and is stable to air and water, especially good stability in water; in addition, the solid electrolyte material has high ionic conductivity and long cycle time.

[0030] According to some embodiments of the present invention, preferably, the solid electrolyte material has a structure shown in Formula I:

[0031] Li 6-δ M 1 α Ln3Z 2-β1-β2 M 2 β1 M 3 β2 P γ O 12 Formula I;

[0032] Among them, -1<δ<1, 0.15<α<0.5, 0≤β1<1, 0≤β2<1, 0<γ<1, and 0<β1+β2<2;

[0033] M 1 Selected from Al and / or Ga;

[0034] M 2 At least one selected from Y, Co, Ti, Sn, Ge and Hf;

[0035] M 3 At least one selected from the group consisting of Mo, W, Sb, Nb and Ta.

[0036] By adopting the above preferred embodiment, the stability of cubic phase LLZO in air and water can be effectively improved through doping. Among them, phosphorus doping can regulate the O-Zr-O bond angle and stabilize the crystal structure; Zr-site doping can regulate the O-Zr-O bond length, strengthen the stability of the ZrO6 octahedron, and thus improve the stability of the cubic phase LLZO. In addition, multi-site doping at the Zr position can effectively improve the stability of the cubic phase LLZO in air and water. Moreover, multi-element synergistic doping can also improve the ionic conductivity of the solid electrolyte material and the ability to inhibit lithium dendrites.

[0037] According to some embodiments of the present invention, preferably, in Formula I, 0.02<γ<0.6, 0.02<β1+β2<0.8; more preferably, 0.03<β1+β2<0.6. The above embodiments are advantageous for further improving the crystal structure stability, ionic conductivity and ability to inhibit lithium dendrites of the solid electrolyte material.

[0038] According to some embodiments of the present invention, preferably, the solid electrolyte material comprises hollow particles with porous surfaces, and the D 50 The diameter is 2-30μm, and the surface porosity is 20%-80%.

[0039] The hollow particles in the present invention include particles that are completely hollow inside, such as Figure 3 As shown, the wall thickness of the outer shell of the particle is 0.5-5 μm; it also includes particles with internal support structures, such as Figure 4 As shown, the wall thickness of the outer shell layer of the particle and the thickness of the supporting structure are both 0.5-5 μm.

[0040] By adopting the above preferred embodiment, the hollow structure particles with holes on the surface are easy to be crushed to obtain nanomaterials, which is beneficial to the nano-sizing of solid electrolyte materials.

[0041] A second aspect of the present invention provides a method for preparing the solid electrolyte material according to the first aspect, the method comprising the following steps:

[0042] (1) In the presence of a solvent, a lithium source, a lanthanum source, a zirconium source, a phosphorus source and M 1 The source is mixed and ground, and the obtained product is dried to obtain a mixed material; wherein the mixed material also contains M 2 Source and / or M 3 Source: D of the mixture 50 <0.5μm, D 100 <1μm;

[0043] (2) In a dry atmosphere, the mixed material is sequentially sintered, crushed, sieved and iron-removed.

[0044] The inventors of the present invention have found in the course of research that the method can obtain a highly reactive mixture by wet grinding and drying through the coordinated doping of multi-site elements, and the particle size of the mixture meets the above-mentioned specific range. 50 Control, combined with subsequent sintering and other operations, can obtain a cubic garnet-type solid electrolyte material, and effectively regulate the O-Zr-O bond length and O-Zr-O bond angle of the solid electrolyte material to improve its crystal structure stability, stability to air and water, especially good stability in water, which is conducive to obtaining a high-performance solid electrolyte.

[0045] According to some embodiments of the present invention, preferably, in step (1), D of the mixture A 50 <0.3μm, D 100 The above preferred implementation is beneficial to further improve the crystal structure stability, ion conductivity and ability to inhibit lithium dendrites of the solid electrolyte material.

[0046] According to some embodiments of the present invention, preferably, in step (1), the solvent is selected from water and / or ethanol, preferably water. Using water as a wet grinding medium can reduce the cost of nano-grinding.

[0047] According to some embodiments of the present invention, preferably, in step (1), the mixed raw materials also include a dispersant, and the dispersant is selected from at least one of polyethylene glycol, polyethylene, polypropylene, sodium polyacrylate and polyvinyl alcohol. The above preferred embodiment is conducive to reducing grain boundaries and improving the ionic conductivity of the solid electrolyte material.

[0048] Preferably, the mass ratio of the dispersant to the mixed material is 0.5-1:100.

[0049] According to some embodiments of the present invention, preferably, in step (1), the drying treatment is carried out by spray drying; the conditions of the drying treatment include: an inlet air temperature of 180-220°C and an outlet air temperature of 95-100°C.

[0050] According to some embodiments of the present invention, preferably, in step (1), the M 1 Source, the M 2 Source and the M 3 The sources are each independently selected from at least one of oxides, hydroxides, carbonates, oxalates, acetates and citrates containing M, wherein M is M 1 、M 2 and M 3 For example, the M 1 The source is selected from the 1At least one of oxides, hydroxides, carbonates, oxalates, acetates and citrates; said M 2 The source is selected from the 2 At least one of oxides, hydroxides, carbonates, oxalates, acetates and citrates; said M 3 The source is selected from the 3 At least one of oxides, hydroxides, carbonates, oxalates, acetates and citrates.

[0051] According to some embodiments of the present invention, preferably, in step (1), the M 1 The source is Al2O3; the M 2 The source is TiO2 and / or GeO2; the M 3 The sources are Nb2O5 and / or WO3.

[0052] According to some embodiments of the present invention, preferably, in step (1), the lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate, preferably lithium carbonate.

[0053] According to some embodiments of the present invention, preferably, in step (1), the ratio of the amount of the lithium source to its stoichiometric amount, calculated as Li, is 1-1.1:1, preferably 1.04-1.1:1, to compensate for lithium volatilization during sintering.

[0054] According to some embodiments of the present invention, preferably, in step (1), the lanthanum source is selected from at least one of lanthanum oxide, lanthanum hydroxide, lanthanum carbonate, lanthanum oxalate, lanthanum acetate and lanthanum citrate.

[0055] According to some embodiments of the present invention, preferably, in step (1), the zirconium source is selected from at least one of zirconium oxide, zirconium hydroxide, zirconium carbonate, zirconium oxalate, zirconium acetate and zirconium citrate.

[0056] According to some embodiments of the present invention, preferably, in step (1), the phosphorus source is selected from at least one of NH4H2PO4, H3PO4 and LiH2PO4.

[0057] According to some embodiments of the present invention, preferably, in step (1), the lithium source, the lanthanum source, the zirconium source, the phosphorus source, the M 1 Source, the M 2 Source and the M 3 The amount of the source is such that the obtained solid electrolyte material has the structure shown in Formula I. The specific structure is as described above and will not be repeated here. 1 Source, the M 2 Source and the M 3The molar amount of the source satisfies the stoichiometric ratio of the structure shown in Formula I.

[0058] According to some embodiments of the present invention, preferably, in step (2), the sintering includes a first stage and a second stage performed sequentially.

[0059] Preferably, the conditions of the first stage include: a heating rate of 0.5-10°C / min, preferably 1-5°C / min; a sintering temperature of 300-700°C, preferably 380-600°C; and a holding time of 0.5-5h, preferably 1.5-3h.

[0060] Preferably, the conditions of the second stage include: a heating rate of 0.5-10°C / min, preferably 1-3°C / min; a sintering temperature of 780-960°C, preferably 850-900°C; and a holding time of 5-24h, preferably 6-12h.

[0061] The above preferred embodiment is beneficial to improve the stability of the crystal structure of the solid electrolyte material. In addition, within the above range, further increasing the sintering temperature can improve the stability of the crystal structure of the solid electrolyte material, reduce the content of lithium hydroxide and lithium carbonate on the surface, and ensure that the solid electrolyte material has a higher ionic conductivity.

[0062] According to some embodiments of the present invention, preferably, in step (2), the dry atmosphere is provided by at least one of dry air, dry oxygen and dry nitrogen.

[0063] According to some embodiments of the present invention, the specific operations of the grinding, crushing, screening (screening), and iron removal are not particularly limited and can be performed with reference to the prior art. In the present invention, the grinding can be achieved by a stirred ball mill, a planetary ball mill, or a sand mill; the crushing can be achieved by a roller crusher, a ball mill, a jet mill, or a mechanical mill; the screening (screening) can be achieved by an ultrasonic vibrating screen; and the iron removal can be achieved by an electromagnetic iron remover.

[0064] A third aspect of the present invention provides a composite solid electrolyte, which comprises the solid electrolyte material described in the first aspect, a lithium salt and a binder.

[0065] According to some embodiments of the present invention, preferably, in the composite solid electrolyte, the mass ratio of the solid electrolyte material, the lithium salt and the binder is 1:0.5-2:1-5.

[0066] According to some embodiments of the present invention, the lithium salt may be a lithium salt suitable for solid-state lithium batteries conventionally used in the art. Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bistrifluoromethylsulfonyl imide (LiTFSI), lithium bisfluorosulfonyl imide, lithium bisoxalatoborate, lithium difluorooxalatoborate and lithium trifluoromethanesulfonate.

[0067] According to some embodiments of the present invention, the binder may be a binder conventionally used in the art and suitable for solid-state lithium batteries. Preferably, the binder is selected from one or more of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, polyethylene oxide (PEO), polyether, polymethyl methacrylate, polyacrylonitrile, polyethylene carbonate and polypropylene carbonate.

[0068] According to some embodiments of the present invention, preferably, the composite solid electrolyte is in the form of a film, and the thickness of the film is 2-30 μm.

[0069] A fourth aspect of the present invention provides a method for preparing the composite solid electrolyte according to the third aspect, the preparation method comprising:

[0070] (1) mixing a solid electrolyte material, a lithium salt and a binder to obtain a mixed product;

[0071] (2) subjecting the kneaded product to hot pressing.

[0072] According to some embodiments of the present invention, preferably, the mixing conditions include: a temperature of 0.5-0.9T m , where T m The mixing time is when the torque of the mixer reaches a steady state.

[0073] According to some embodiments of the present invention, preferably, the hot pressing conditions include: a temperature of 0.5-0.9T m , where T m The pressure of the hot pressing can be adjusted according to the required thickness of the electrolyte membrane.

[0074] A fifth aspect of the present invention provides a solid-state lithium battery, comprising a positive electrode, an electrolyte and a negative electrode, wherein the electrolyte is the composite solid-state electrolyte described in the third aspect.

[0075] The present invention will be described in detail below through examples.

[0076] In the following examples, unless otherwise specified, the raw materials and equipment used are commercially available.

[0077] In the following examples, the relevant parameters are measured by the following method:

[0078] Particle size test: obtained by using Malvern laser particle size analyzer Mastersizer 2000;

[0079] Phase and crystal structure: obtained by testing with Rigaku X-ray automatic diffractometer;

[0080] Bond length and bond angle: calculated by density functional theory and molecular dynamics simulation;

[0081] SEM and wall thickness: obtained using a Japanese Hitachi S-4800 scanning electron microscope;

[0082] Surface porosity: obtained by measuring the projected area of ​​the pores using a Hitachi IM4000plus ion mill and a Hitachi S-4800 scanning electron microscope;

[0083] Ionic conductivity: tested using Bio-logic SP-150 electrochemical workstation;

[0084] Charge and discharge cycle performance: tested using CT-3008 from Xinwei Electronics Co., Ltd.

[0085] The following examples are used to illustrate the solid electrolyte material and the preparation method thereof provided by the present invention.

[0086] Example 1

[0087] (1) In the presence of a solvent, a lithium source (Li2CO3), a lanthanum source (La2O3), a zirconium source (ZrO2), a phosphorus source (NH4H2PO4), and M 1 Source (Al2O3), M 2 Source (TiO2), M 3 The source (Nb2O5) and the dispersant (PEG1500) are mixed and ground, and then the obtained product is dried to obtain a mixed material; wherein:

[0088] D of the above mixture 50 0.2μm, D 100 The molar ratio of each raw material is as follows: n(Li):n(La):n(Zr):n(P):n(Al):n(Nb):n(Ti)=6.60:3:1.93:0.03:0.2:0.02:0.02, wherein the molar amount of the lithium source calculated as Li is 4% more than the theoretical value;

[0089] The solvent is water; the mass ratio of the dispersant to the above-mentioned mixture is 0.5:100;

[0090] The drying method is spray drying; the inlet air temperature of spray drying is 200°C and the outlet air temperature is 97°C;

[0091] (2) In a dry atmosphere, the mixed material is placed in a roller kiln for sintering, crushing, screening and iron removal in sequence; wherein:

[0092] The dry atmosphere is provided by dry air; the sintering is carried out in sequence in the first stage and the second stage;

[0093] The conditions of the first stage are: heating rate 5℃ / min; sintering temperature 520℃; holding time 3h;

[0094] The conditions of the second stage include: heating rate of 2°C / min; sintering temperature of 850°C; holding time of 8h;

[0095] After sintering, the sintered product was naturally cooled to 100 °C, and then crushed, sieved and iron-removed to obtain a solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 1.93 Nb 0.02 Ti 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0096] X-ray diffraction test shows that the crystal structure of the X-ray diffraction pattern of the solid electrolyte material is consistent with the cubic phase LLZO standard card PDF#01-090-2617, such as Figure 1 As shown, it is shown that the solid electrolyte material has a cubic garnet-type crystal structure.

[0097] Figure 2 This is a scanning electron microscope image of the solid electrolyte material. It can be seen from the image that there is basically no residual impurities such as lithium carbonate on the surface of the solid electrolyte material, which is conducive to lithium ion transmission and has high stability.

[0098] Figure 3 and Figure 4 is a cross-sectional view of the solid electrolyte material. It can be seen from the figure that the particles of the solid electrolyte material are hollow particles with porous surfaces.

[0099] Example 2

[0100] The method of Example 1 is different from that of Example 1:

[0101] In step (1), M 3 The source is WO3; the molar ratio of each raw material is: n(Li):n(La):n(Zr):n(P):n(Al):n(W):n(Ti)=6.58:3:1.93:0.03:0.2:0.02:0.02;

[0102] The rest are the same, and the solid electrolyte material (Li 6.33 Al 0.2 Ln3Z 1.93 W 0.02 Ti 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0103] Example 3

[0104] The method of Example 1 is different from that of Example 1:

[0105] In step (1), M 2 The source is GeO2; the molar ratio of the raw materials is: n(Li):n(La):n(Zr):n(P):n(Al):n(Nb):n(Ge)=6.60:3:1.93:0.03:0.2:0.02:0.02, wherein the molar amount of the lithium source calculated as Li is 4% more than the theoretical value;

[0106] The rest are the same, and the solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 1.93 Nb 0.02 Ge 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0107] Example 4

[0108] The method of Example 1 is used, except that in step (1), the molar ratio of the raw materials is as follows: n(Li):n(La):n(Zr):n(P):n(Al):n(Nb):n(Ti)=6.58:3:1.91:0.05:0.2:0.02:0.02, wherein the molar amount of the lithium source calculated as Li is 4% in excess of the theoretical value;

[0109] The rest are the same, and the solid electrolyte material (Li 6.33 Al 0.2 Ln3Z 1.91 Nb 0.02 Ti 0.02 P 0.05 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0110] Example 5

[0111] The method of Example 1 is used, except that in step (1), the molar ratio of the raw materials is as follows: n(Li):n(La):n(Zr):n(P):n(Al):n(Nb):n(Ti)=6.62:3:1.9:0.01:0.2:0.02:0.02, wherein the molar amount of the lithium source calculated as Li is 4% in excess of the theoretical value;

[0112] The rest are the same, and the solid electrolyte material (Li 6.37 Al 0.2 Ln3Z 1.95 Nb 0.02 Ti 0.02 P 0.01 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0113] Example 6

[0114] The method of Example 1 is followed, except that in step (1), the molar ratio of the raw materials is as follows: n(Li):n(La):n(Zr):n(P):n(Al):n(Nb):n(Ti)=6.60:3:0.97:0.03:0.2:0.02:0.78, wherein the molar amount of the lithium source calculated as Li is 4% in excess of the theoretical value;

[0115] The rest are the same, and the solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 0.97 Nb 0.02 Ti 0.78 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0116] Example 7

[0117] The method of Example 1 is different from that of Example 1:

[0118] In step (2), the sintering temperature of the second stage is 780°C;

[0119] The rest are the same, and the solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 1.93 Nb 0.02 Ti 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0120] Example 8

[0121] The method of Example 1 is different from that of Example 1:

[0122] In step (2), the sintering temperature of the second stage is 950°C;

[0123] The rest are the same, and the solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 1.93 Nb 0.02 Ti 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0124] Example 9

[0125] The method of Example 1 is followed, except that in step (1), D of the mixture is 50 =0.1μm, D 100 =0.5μm; the rest are the same, and a solid electrolyte material is obtained; its basic physicochemical parameters are shown in Table 1.

[0126] Example 10

[0127] The method of Example 1 is different from that of Example 1:

[0128] In step (1), the mixed raw materials do not contain M 3 Source, the molar ratio of each raw material meets the following requirements: n(Li):n(La):n(Zr):n(P):n(Al):n(Ti)=6.60:3:1.95:0.03:0.2:0.02, wherein the molar amount of lithium source calculated as Li is 4% more than the theoretical value;

[0129] The rest are the same, and the solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 1.95 Ti 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0130] Embodiment 11

[0131] The method of Example 1 is different from that of Example 1:

[0132] In step (1), the mixed raw materials do not contain M 2 Source, the molar ratio of each raw material meets the following requirements: n(Li):n(La):n(Zr):n(P):n(Al):n(Nb)=6.62:3:1.97:0.03:0.2:0.02, wherein the molar amount of lithium source calculated as Li is 4% more than the theoretical value;

[0133] The rest are the same, and the solid electrolyte material (Li 6.37Al 0.2 Ln3Z 1.97 Nb 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0134] Comparative Example 1

[0135] The method of Example 1 is followed, except that in step (1), the mixed raw materials do not contain solvent, phosphorus source, M 1 Source, M 2 Source, M 3 Source, dispersant, as follows:

[0136] (1) mixing and grinding a lithium source (Li2CO3), a lanthanum source (La2O3) and a zirconium source (ZrO2) to obtain a mixed material; the molar ratio of the raw materials is as follows: n(Li):n(La):n(Zr)=7.28:3:2, wherein the molar amount of the lithium source calculated as Li is 4% in excess of the theoretical value;

[0137] (2) The same as step (2) of Example 1, to obtain a solid electrolyte material (Li7La3Zr2O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0138] X-ray diffraction tests show that there are a large number of splitting peaks in the X-ray diffraction pattern of the solid electrolyte material, such as Figure 1 As shown, it is a tetragonal crystal structure.

[0139] Figure 5 This is a scanning electron microscope image of the solid electrolyte material. It can be seen from the image that there are a large number of impurities such as lithium carbonate on the surface of the solid electrolyte material, which is not conducive to lithium ion transmission and has poor stability.

[0140] Figure 6 is a cross-sectional view of the solid electrolyte material. It can be seen from the figure that the interior of the particles of the solid electrolyte material is a solid structure and there are no holes on the surface of the particles.

[0141] Comparative Example 2

[0142] The method of Example 1 is different from that of Example 1:

[0143] In step (1), the mixed raw materials do not contain a phosphorus source; the molar ratio of the raw materials is as follows: n(Li):n(La):n(Zr):n(Al):n(Nb):n(Ti)=6.64:3:1.93:0.2:0.02:0.02, wherein the molar amount of the lithium source calculated as Li is 4% in excess of the theoretical value;

[0144] The rest are the same, and the solid electrolyte material (Li6.38 Al 0.2 Ln3Z 1.96 Nb 0.02 Ti 0.02 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0145] Comparative Example 3

[0146] The method of Example 1 is different from that of Example 1:

[0147] In step (1), the mixed raw materials do not contain M 2 Source and M 3 Source; the molar ratio of each raw material satisfies: n(Li):n(La):n(Zr):n(P):n(Al)=6.62:3:1.97:0.03:0.2, wherein the molar amount of the lithium source calculated as Li is 4% in excess of the theoretical value;

[0148] The rest are the same, and the solid electrolyte material (Li 6.37 Al 0.2 Ln3Z 1.97 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0149] Comparative Example 4

[0150] The method of Example 1 is different from that of Example 1:

[0151] In step (1), the D 50 =1.1μm, D 100 =3.2μm; the rest are the same, and the solid electrolyte material (Li 6.35 Al 0.2 Ln3Z 1.93 Nb 0.02 Ti 0.02 P 0.03 O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0152] Comparative Example 5

[0153] The method of Example 1 is followed, except that in step (1):

[0154] There is no M in the mixed raw materials 1 Source, M 2 Source, M 3 Source and phosphorus source; the molar ratio of each raw material is as follows: n(Li):n(La):n(Zr)=7.28:3:2;

[0155] D of the mixture 50=1.1μm, D 100 =3.2μm;

[0156] The rest are the same, and the solid electrolyte material (Li7La3Zr2O 12 ); its basic physical and chemical parameters are shown in Table 1.

[0157] Table 1

[0158]

[0159]

[0160] Test Example 1

[0161] The solid electrolyte materials prepared in the embodiment and the comparative example were respectively ball-milled in water, and the specific steps were as follows: the solid electrolyte material, PEG1500, water and 0.2 mm zirconium ball were ball-milled according to a mass ratio of 100:0.5:240:500, the ball milling speed was 500 rpm, and the ball milling time was 5 hours. Samples were taken every 1 hour, and the crystal structure of the powder was tested after drying at 120°C. The test results of the change of the crystal structure with the ball milling time are shown in Table 2.

[0162] The present invention exemplarily provides X-ray diffraction patterns of the solid electrolyte materials prepared in Example 1, Example 10 and Comparative Examples 2-3 after ball milling in water for 300 minutes and drying, as shown in FIG. Figure 7 shown.

[0163] Table 2

[0164]

[0165]

[0166] Note: c-LLZO represents cubic phase LLZO, and t-LLZO represents tetragonal phase LLZO.

[0167] pass Figure 7 As can be seen from the above results: By comparing the schemes and effects of Example 1 with those of Comparative Examples 2-3, it can be seen that after ball milling in water, the crystal structure of the sample in the comparative example changes from cubic LLZO to a mixed phase of cubic LLZO and La(OH)3, and finally to La(OH)3 phase, while the sample in Example 1 can maintain a complete crystal structure. This shows that doping can effectively improve the stability of cubic LLZO in water. Among them, phosphorus doping can regulate the O-Zr-O bond angle and stabilize the crystal structure; Zr doping can regulate the O-Zr-O bond length, strengthen the stability of the ZrO6 octahedron, and thus improve the stability of the cubic LLZO.

[0168] By comparing the schemes and effects of Example 1 with those of Examples 10-11, it can be seen that the La(OH)3 phase appeared in the sample of Example 10-11 after ball milling for 300 minutes, indicating that multi-site doping at the Zr position can effectively improve the stability of the cubic phase LLZO in water.

[0169] Test Example 2

[0170] The solid electrolyte materials prepared in the embodiments and comparative examples were exposed to the air for 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 24 h, 48 h, 72 h, 96 h, and 120 h, respectively, and samples were taken. The contents (weight %) of residual lithium carbonate and lithium hydroxide on the surface of the powders were tested by titration with hydrochloric acid. The test results of the changes in the total amount of residual lithium carbonate and lithium hydroxide with exposure time are shown in Table 3.

[0171] Table 3

[0172]

[0173]

[0174] It can be seen from the above results that, by comparing the schemes and effects of Example 1 with Comparative Examples 2-3, it can be seen that after the solid electrolyte material provided by the present invention is exposed to the air, less lithium hydroxide and lithium carbonate are generated on the surface, indicating that the O-Zr-O bond length and O-Zr-O bond angle can be regulated by doping, the crystal structure can be stabilized, and the air stability can be improved.

[0175] By comparing the schemes and effects of Example 1 with Example 7, it can be seen that after the solid electrolyte material obtained in Example 7 is exposed to air for 24 hours and 120 hours, the surface lithium hydroxide and lithium carbonate are more, that is, it is easier to react with carbon dioxide and moisture in the air, indicating that the sintering temperature is within the preferred range of the present invention, which is conducive to improving the stability of its crystal structure. In addition, within the scope defined by the present invention, increasing the sintering temperature can improve the stability of the crystal structure of the solid electrolyte material, reduce the surface lithium hydroxide and lithium carbonate (Example 8), and ensure that it has a higher ionic conductivity.

[0176] By comparing the schemes and effects of Example 1 with those of Examples 10-11, it can be seen that after Example 10-11 was exposed to the air for 24 hours and 120 hours, more lithium hydroxide and lithium carbonate were present on the surface, indicating that the synergistic doping of multiple elements can better improve the stability of the solid electrolyte material in the air.

[0177] Test Example 3

[0178] The solid electrolyte materials prepared in the embodiment and the comparative example are respectively assembled into a test system, and the specific steps are as follows:

[0179] The solid electrolyte material, LiTFSI and binder PEO were mixed in a mass ratio of 1:1:3 to obtain a mixed product, which was then hot-pressed to form a film with a thickness of 30 μm. The film was then cut into electrolyte membranes with a diameter of 19 mm, dried in a vacuum at 60°C for 10 hours, and then vacuum-sealed for storage.

[0180] The electrolyte membrane was assembled into a stainless steel|electrolyte|stainless steel test system and a metal lithium|electrolyte|metal lithium test system in a glove box filled with argon gas with a water content and an oxygen content of less than 5 ppm. The stainless steel|electrolyte|stainless steel test system was tested for ion conductivity, and the metal lithium|electrolyte|metal lithium test system was tested for charge and discharge. The test results are shown in Table 4.

[0181] Table 4

[0182]

[0183]

[0184] It can be seen from the above results that: by comparing the schemes and effects of Example 1 with those of Comparative Example 1, it can be seen that the ionic conductivity of the cubic phase LLZO is significantly higher than that of the tetragonal phase LLZO.

[0185] By comparing the schemes and effects of Example 1 with those of Examples 7-8, it can be seen that after a suitable sintering temperature, a crystal structure with a specific bond length and angle can be obtained, the lithium ion transmission channel can be optimized, and a higher ion conductivity can be obtained. At too low a sintering temperature, the continuity of the lithium ion channel is incomplete; at too high a sintering temperature, the unit cell size is reduced, the lithium ion channel becomes smaller, and the difficulty of ion transmission is increased.

[0186] By comparing the schemes and effects of Example 1 with those of Examples 10-11, it can be seen that the ionic conductivity of the solid electrolyte material obtained in Example 1 is 1.28 times that of the solid electrolyte material of Examples 10-11, indicating that multi-element synergistic doping can improve the ionic conductivity of the solid electrolyte material.

[0187] By comparing the schemes and effects of Example 1 with those of Comparative Examples 2-3, it can be seen that the solid electrolyte material provided by the present invention has a longer cycle time, that is, the lithium ion flow distribution during the cycle is more uniform, indicating that it can better inhibit lithium dendrites.

[0188] By comparing the schemes and effects of Example 1 and Comparative Example 4, it can be seen that in the preparation process of the solid electrolyte material, the D 50 It has a great influence on the ionic conductivity and cycle time of the prepared solid electrolyte material. 50 When it is too large, the grain boundaries in the sintered solid electrolyte material are thick, which is not conducive to the uniform conduction of lithium ions.

[0189] Comparing Example 1 with Example 9, it can be seen that in the mixture D defined in the present invention 50 Within the range, D 50 Further reduction (Example 9) can further improve the ionic conductivity of the solid electrolyte material and the ability to inhibit lithium dendrites.

[0190] In addition, no doping, mixed material D 50 The solid electrolyte material obtained by over-sintering (Comparative Example 5) has very low ion conductivity and a very short cycle time.

[0191] In summary, the solid electrolyte material provided by the present invention has a stable crystal structure, high ion conductivity, and a long cycle time. In a preferred case, the method provided by the present invention can effectively reduce the synthesis temperature of the cubic garnet-type solid electrolyte material, and the particles are easy to nanosize.

[0192] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A solid electrolyte material, It is characterized in that The solid electrolyte material has a structure shown in Formula I: Li 6-δ M 1 α La 3 Zr 2-β1-β2 M 2 β1 M 3 β2 P γ O 12 Formula I; Among them, -1<δ<1, 0.15<α<0.5, 0≤β1<1, 0≤β2<1, 0<γ<1, and 0<β1+β2<2; M 1 Selected from Al and / or Ga; M 2 At least one selected from Y, Co, Ti, Sn, Ge and Hf; M 3 At least one selected from Mo, W, Sb, Nb and Ta; The crystal structure of the solid electrolyte material satisfies: the O-Zr-O bond length is or The O-Zr-O bond angle is 176.30°-179.97° or 180.03°-183.70°.

2. The solid electrolyte material according to claim 1, in, 0.02<γ<0.6, 0.02<β1+β2<0.

8.

3. The solid electrolyte material according to claim 2, in, 0.03<β1+β2<0.6。 4. The solid electrolyte material according to any one of claims 1 to 3, in, The solid electrolyte material comprises hollow particles with porous surfaces, wherein the D 50 The diameter is 2-30μm, and the surface porosity is 20%-80%.

5. A method for preparing the solid electrolyte material according to any one of claims 1 to 4, the method comprising the following steps: (1) In the presence of a solvent, a lithium source, a lanthanum source, a zirconium source, a phosphorus source, a dispersant and M 1 The sources are mixed and ground, and then the obtained product is dried to obtain a mixture A; in, The mixture also contains M 2 Source and / or M 3 Source: D of the mixture 50 <0.5μm, D 100 <1μm; (2) In a dry atmosphere, the mixed material is sequentially sintered, crushed, sieved and iron-removed.

6. The method according to claim 5, in, In step (1), the mixture A has D 50 <0.3μm, D 100 <0.8μm.

7. The method according to claim 5, in, The solvent is selected from water and / or ethanol.

8. The method according to claim 7, in, The solvent is water.

9. The method according to claim 5, in, The dispersant is selected from at least one of polyethylene glycol, polyethylene, polypropylene, sodium polyacrylate and polyvinyl alcohol; the mass ratio of the dispersant to the mixed material is 0.5-1:

100.

10. The method according to claim 5, in, The drying method is spray drying; the drying conditions include: an inlet air temperature of 180-220°C and an outlet air temperature of 95-100°C.

11. The method according to any one of claims 5 to 10, in, In step (1), the M 1 Source, the M 2 Source and the M 3 The sources are each independently selected from at least one of oxides, hydroxides, carbonates, oxalates, acetates and citrates containing M, wherein M is M 1 、M 2 and M 3 At least one of; And / or, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate; and / or, the lanthanum source is selected from at least one of lanthanum oxide, lanthanum hydroxide, lanthanum carbonate, lanthanum oxalate, lanthanum acetate and lanthanum citrate; And / or, the zirconium source is selected from at least one of zirconium oxide, zirconium hydroxide, zirconium carbonate, zirconium oxalate, zirconium acetate and zirconium citrate; And / or, the phosphorus source is selected from NH 4 H 2 PO 4 , H 3 PO 4 and LiH 2 PO 4 At least one of .

12. The method according to any one of claims 5 to 10, in, In step (1), the ratio of the amount of the lithium source to its stoichiometric amount is 1-1.1:1, calculated as Li.

13. The method according to claim 12, in, In step (1), the ratio of the amount of the lithium source to its stoichiometric amount is 1.04-1.1:1, calculated as Li.

14. The method according to any one of claims 5 to 10, in, In step (2), the sintering includes a first stage and a second stage which are performed sequentially.

15. The method according to claim 14, in, The conditions of the first stage include: heating rate of 0.5-10°C / min; sintering temperature of 300-700°C; and holding time of 0.5-5h.

16. The method according to claim 15, in, The heating rate is 1-5℃ / min; the sintering temperature is 380-600℃; and the holding time is 1.5-3h.

17. The method according to claim 14, in, The conditions of the second stage include: heating rate of 0.5-10°C / min; sintering temperature of 780-960°C; and holding time of 5-24h.

18. The method according to claim 17, in, The heating rate is 1-3℃ / min; the sintering temperature is 850-900℃; and the holding time is 6-12h.

19. A composite solid electrolyte, It is characterized in that The composite solid electrolyte comprises the solid electrolyte material according to any one of claims 1 to 4, a lithium salt and a binder.

20. The composite solid electrolyte according to claim 19, in, In the composite solid electrolyte, the mass ratio of the solid electrolyte material, the lithium salt and the binder is 1:0.5-2:1-5.

21. The composite solid electrolyte according to claim 19, in, The composite solid electrolyte is in the form of a film, and the thickness of the film is 2-30 μm.

22. A method for preparing the composite solid electrolyte according to any one of claims 19 to 21, wherein the preparation method include: (1) mixing a solid electrolyte material, a lithium salt and a binder to obtain a mixed product; (2) subjecting the kneaded product to hot pressing.

23. The preparation method according to claim 22, in, The mixing conditions include: a temperature of 0.5-0.9T m ; And / or, the hot pressing conditions include: a temperature of 0.5-0.9T m ; Among them, T m is the melting point of the binder.

24. A solid-state lithium battery, comprising a positive electrode, an electrolyte and a negative electrode, It is characterized in that The electrolyte is a composite solid electrolyte as described in any one of claims 19-21.

Citation Information

Patent Citations

  • Nb and Ta co-doped garnet-type LLZO solid electrolyte and preparation method thereof

    CN109935901A

  • Cubic phase garnet type solid electrolyte material, composite solid electrolyte, solid lithium battery and preparation method of solid lithium battery

    CN114497710A

  • Solid electrolyte material, preparation method thereof and lithium ion solid-state battery

    CN115882055A