A composite short fiber reinforced composite material and preparation method thereof

Through graphene oxide grafting technology and epoxy end-capped hyperbranched polyamide functional components, the problem of poor compatibility between carbon fiber and nylon resin is solved, the mechanical properties and flame retardancy of composite materials are improved, and good processing performance is achieved and water resistance.

CN117887248BActive Publication Date: 2024-11-12ANHUI TONGLI NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410151634.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-02
Publication Date
2024-11-12
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

Poor compatibility between carbon fiber and nylon resin leads to poor interfacial bonding, affecting the mechanical properties of the composite material.

Method used

Graphene oxide grafting technology is used to deposit graphene oxide on the surface of carbon fiber to increase its surface activity and wettability, and use epoxy capped hyperbranched polyamide as a functional component to improve the compatibility of carbon fiber and nylon 6. and mechanical properties.

Benefits of technology

It improves the wetting and mechanical meshing of carbon fiber and nylon resin, enhances the mechanical properties and processing rheology of the composite material, and imparts good flame retardant and water resistance to the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a composite short fiber reinforced composite material, belongs to the technical field of nylon composite materials, comprises the following raw materials by weight: 60-70 parts of nylon 6, 15-30 parts of composite short fibers, 3-7 parts of functional components, 0.2-1 parts of lubricants and 0.4-1 parts of antioxidants, wherein the composite short fibers are graphene oxide grafted short chopped carbon fibers. The invention also discloses a preparation method of the composite short fiber reinforced composite material, which is simple to prepare, has good wettability and mechanical meshing between the composite short fibers and the nylon resin, and can give full play to the reinforcing effect; the functional components can improve the processing rheology and internal transmission of stress of the composite material, and are nitrogen- and phosphorus-containing organic substances, which can improve the flame retardant properties of the composite material; in addition, the functional components also contain fluorocarbon chains, have strong hydrophobicity, and are conducive to improving the water resistance of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nylon composite materials, and particularly relates to a composite short fiber reinforced composite material and a preparation method thereof. Background Art

[0002] Polyamide (PA), commonly known as nylon, is an important engineering plastic with high temperature resistance, wear resistance and high mechanical properties. Among them, PA6 is one of the most widely used aliphatic polyamides, but as an engineering material, the rigidity and strength of PA6 are still far behind those of metals. For this reason, glass fiber is used to reinforce PA6 and improve the mechanical properties of PA6 materials. It has been widely used, but the density of glass fiber is relatively large, and the density of the composite material obtained by reinforcement and modification also increases, resulting in a decrease in the market competitiveness of the product. In order to further improve the performance of modified PA6 composite materials and make them meet the application in higher performance fields, the use of carbon fiber to reinforce PA6 composite materials has become a current research hotspot.

[0003] Carbon fiber has high specific strength, high specific modulus, excellent anti-damping performance and chemical corrosion resistance, but its surface is chemically inert and lacks active chemical groups. PA6 has high relative viscosity and poor melt fluidity, which makes it difficult to impregnate carbon fiber, resulting in poor interface bonding between the two. To this end, this problem is currently solved by surface modification of carbon fiber. There are two main methods. One is surface oxidation method, which uses strong oxidizing liquid, gas phase, and plasma oxidation to introduce active oxygen-containing functional groups on the fiber surface. Although there are advantages of short reaction time and good modification effect, it is easy to lose fiber structure, resulting in a decrease in carbon fiber strength and poor reinforcement effect; the second is surface chemical coating method, which coats the carbon fiber surface with a commercial sizing agent, mostly epoxy resin polymers, as described in patent CN108503865B. Although certain technical effects are achieved, the epoxy sizing agent has poor compatibility with the thermoplastic resin matrix, which is not conducive to the interface performance of thermoplastic composite materials, resulting in unsatisfactory improvement in the mechanical properties of composite materials. Therefore, how to improve the compatibility between carbon fiber and nylon resin is a technical problem that needs to be solved at present. Summary of the invention

[0004] The purpose of the present invention is to provide a composite short fiber reinforced composite material and a preparation method thereof, and to analyze the compatibility problem between carbon fiber and nylon resin.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A composite staple fiber reinforced composite material comprises the following raw materials in parts by weight: 60-70 parts of nylon 6, 15-30 parts of composite staple fibers, 3-7 parts of functional components, 0.2-1 parts of lubricants and 0.4-1 parts of antioxidants.

[0007] The method for preparing the composite short fiber reinforced composite material comprises the following steps:

[0008] Weigh the raw materials according to the weight ratio, put nylon 6, functional components, lubricants and antioxidants into a high-speed mixer and mix for 3-5 minutes to obtain component one, feed component one into a twin-screw extruder through a main feeder, add composite staple fibers into the side feeder of the twin-screw extruder, and perform extrusion, cooling, pelletizing and drying.

[0009] Furthermore, the twin-screw extruder has a rotation speed of 300-400 rpm and a temperature of 220-280°C.

[0010] The composite staple fibers are graphene oxide grafted chopped carbon fibers.

[0011] Furthermore, the steps of preparing the composite staple fiber are as follows:

[0012] Graphene oxide was ultrasonically dispersed in deionized water to obtain a suspension a, short-cut carbon fibers were added to the suspension a, and after ultrasonic dispersion, the pH value was adjusted to 10 with sodium hydroxide to obtain a mixed solution b, two electrodes were inserted into the mixed solution b and the distance between them was adjusted to 1 cm, and the mixture was operated at a constant voltage of 30 V for 1 hour. Finally, the composite staple fibers were separated and dried by a centrifuge.

[0013] Furthermore, the concentration of graphene oxide in the suspension a is 2 mg / mL, the amount ratio of the suspension a to the chopped carbon fiber is 30-50 mL: 3 g, and the chopped carbon fiber is high-carbon glue-free carbon fiber chopped strands.

[0014] In order to solve the problem of high chemical inertness of carbon fiber surface, the present invention grafts graphene oxide onto the surface of carbon fiber by electrophoretic deposition method, and improves the surface polarity of carbon fiber by means of abundant hydroxyl, carboxyl and epoxy groups of graphene oxide, and at the same time improves the surface roughness and wettability of carbon fiber, increases the wettability and mechanical meshing between carbon fiber and nylon resin, and enables carbon fiber to fully exert its reinforcing effect. This treatment method will not damage the carbon fiber itself and does not require sizing treatment. During the shearing process, it can effectively reduce the shearing effect of the screw on the carbon fiber, retain the fiber length, and is more conducive to improving the mechanical properties of the composite material.

[0015] Further, the functional component preparation steps are as follows:

[0016] Step S1, adding tri(3-aminophenyl)phosphine oxide, fluorine-containing carbon branched dicarboxylic acid, N-methylpyrrolidone and pyridine into a flask, protecting with nitrogen, stirring at room temperature for 5-10 minutes, adding triphenyl phosphite, reacting at 20° C. for 2 hours, then heating to 70° C. for 2 hours, and finally heating to 130° C. for 8 hours. After the reaction is completed, the reaction solution is precipitated and filtered in water, washed, and dried to obtain a hyperbranched polyamide;

[0017] Step S2, adding hyperbranched polyamide and anhydrous methanol into a flask, stirring and then dripping 3,4-dihydroxybenzaldehyde methanol solution into the flask, and after the dripping is completed, reacting at 60° C. for 6 hours under nitrogen protection. After the reaction is completed, pouring the reaction product into ice water, filtering, washing the filter cake with distilled water and drying to obtain Schiff base hyperbranched polyamide;

[0018] Step S3, add Schiff base hyperbranched polyamide, potassium hydroxide and anhydrous ethanol into a flask, stir to dissolve, then add epichlorohydrin, react at 70°C for 4 hours under nitrogen protection, cool to room temperature, dropwise add potassium hydroxide aqueous solution, after the dropwise addition is completed, stir and react at 60°C for 6 hours, then cool to room temperature, filter, and evaporate the filtrate to remove anhydrous ethanol and water to obtain functional components.

[0019] The invention discloses a hyperbranched polyamide prepared by an A2+B3 method using tri(3-aminophenyl)phosphine oxide as a B3 monomer and a fluorine-containing carbon branched dicarboxylic acid as an A2 monomer, and then obtaining a Schiff base hyperbranched polyamide containing a phenolic hydroxyl group by a condensation reaction between an amino group and an aldehyde group, and finally obtaining a functional component by epoxy functionalization of the phenolic hydroxyl group using epichlorohydrin; the functional component is a hyperbranched polymer, and the presence of a highly branched structure reduces the size of the polymer molecule, weakens the mutual entanglement of the molecular chains, has the characteristics of low melt viscosity and high fluidity, has good compatibility with nylon resin, and numerous epoxy groups at the end can react with the terminal amino group and the terminal carboxyl group of nylon 6 at the same time, thereby increasing the molecular weight of nylon 6 and It promotes the branching of nylon 6 molecular chains, improves the processing rheology of composite materials and the internal transmission of stress, and ultimately significantly improves the melt index and mechanical properties of the composite materials. Since the functional component contains phosphorus-containing organic matter with a Schiff base structure, at high temperatures, the C=N double bonds can be cross-linked to form a carbon-nitrogen six-membered ring, giving the material excellent carbon-forming properties. After thermal decomposition, it is easy to produce phosphoric acid, metaphosphoric acid or polymetaphosphoric acid, which promotes the rapid dehydration and carbonization of organic matter, promotes carbonization, and produces non-flammable gases such as amino and nitrogen. By absorbing heat and diluting the concentration of combustible gases, the flame retardant properties of the composite materials are improved. In addition, the functional component also contains fluorocarbon chains, which have strong hydrophobicity and are beneficial to improving the water resistance of the composite materials.

[0020] Furthermore, in step S1, the usage ratio of tri(3-aminophenyl)phosphine oxide, fluorine-containing carbon branched dicarboxylic acid, N-methylpyrrolidone, pyridine and triphenyl phosphite is 1.1-1.2 g: 2.2 g: 20 mL: 5 mL: 5 mL.

[0021] Furthermore, in step S2, the mass ratio of the hyperbranched polyamide to 3,4-dihydroxybenzaldehyde is 10:1-4.

[0022] Furthermore, in step S3, the dosage ratio of Schiff base hyperbranched polyamide, potassium hydroxide, anhydrous ethanol, epichlorohydrin and potassium hydroxide aqueous solution is 10g:0.5g:100mL:9.2g:5.6-8.4g, and the mass fraction of potassium hydroxide aqueous solution is 40%.

[0023] Furthermore, the preparation steps of the fluorine-containing carbon branched dicarboxylic acid are as follows:

[0024] Step A1, diallylamine, DMAP and DMF are added into a flask, and after mixing evenly, perfluoroheptanoyl chloride is added dropwise. After the addition is completed, the mixture is stirred at 100° C. for 8-10 hours. After the reaction is completed, DMF is removed by distillation under reduced pressure, the distillation product is washed with water, and the organic phase is dried to obtain an intermediate product;

[0025] Step A2: add the intermediate product, thioglycolic acid, benzoin dimethyl ether and DMF into a flask, stir and place under ultraviolet light to react for 30 minutes, and remove DMF by reduced pressure distillation to obtain a fluorine-containing carbon branched dicarboxylic acid.

[0026] First, diallylamine and perfluoroheptanoyl chloride are subjected to substitution reaction to introduce a branched double bond into the end of the perfluoroheptanoyl chloride to obtain an intermediate product. Then, the double bond of the intermediate product is reacted with a thiol group to introduce a carboxyl group into the molecular chain of the intermediate product to obtain a fluorine-containing carbon branched dicarboxylic acid.

[0027] Furthermore, in step A1, the usage ratio of diallylamine, DMAP, DMF and perfluoroheptanoyl chloride is 0.11-0.12 mol: 0.01 mol: 100-150 mL: 0.1 mol.

[0028] Furthermore, the usage ratio of the intermediate product of step A2, thioglycolic acid, benzoin dimethyl ether and DMF is 4.44 g: 1.8-2.0 g: 0.04-0.06 g: 60-80 mL.

[0029] Furthermore, the lubricant is one or a combination of stearic acid amide, paraffin wax and polyethylene wax.

[0030] Furthermore, the antioxidant is prepared by compounding antioxidant 1010 and antioxidant 168 in a ratio of 1:2.

[0031] Beneficial effects of the present invention:

[0032] The invention provides a composite staple fiber reinforced composite material, which is made of raw materials such as nylon 6, composite staple fibers, functional components, etc., and is simple to prepare. The composite staple fibers are graphene oxide grafted onto carbon fibers, have good wettability and mechanical meshing with nylon resin, and can give full play to the reinforcing effect. The functional component is an epoxy-terminated hyperbranched polymer, and numerous epoxy groups at the ends can react with terminal amino groups and terminal carboxyl groups of nylon 6 at the same time, thereby increasing the molecular weight of nylon 6 and promoting the branching of nylon 6 molecular chains, thereby increasing the processing rheology of the composite material and the internal transmission of stress. The composite material is a nitrogen- and phosphorus-containing organic substance, thereby increasing the flame retardancy of the composite material. In addition, the functional component also contains a fluorocarbon chain, has strong hydrophobicity, and is beneficial to improving the water resistance of the composite material. In summary, the composite material prepared by the invention not only has good processing performance and mechanical properties, but also has good flame retardancy and water resistance. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0035] The PA6 used in this paper, B500F, Nanjing Hongrui Plastic Products Co., Ltd., has a melting temperature of 217°C and a relative viscosity of 3.08;

[0036] The chopped carbon fiber is high carbon glue-free carbon fiber chopped strands with a thickness of 7 μm and a length of 2 mm, purchased from Nanjing Weida Composite Materials Co., Ltd.

[0037] Tris(3-aminophenyl)phosphine oxide was prepared with reference to literature (Hu Mangen, Lai Xiaoping, Zhang Hean, etc., Synthesis of tris(3-aminophenyl)phosphine oxide). Example 1

[0038] The steps for preparing composite staple fibers are as follows:

[0039] Graphene oxide was ultrasonically dispersed in deionized water to obtain a 2 mg / mL suspension a, 3 g of chopped carbon fiber was added to 30 mL of suspension a, and after ultrasonic dispersion, the pH value was adjusted to 10 with sodium hydroxide to obtain a mixed solution b, two electrodes were inserted into the mixed solution b and the distance between them was adjusted to 1 cm, and the mixture was operated at a constant voltage of 30 V for 1 hour. Finally, the composite staple fibers were separated and dried by a centrifuge. Example 2

[0040] The steps for preparing composite staple fibers are as follows:

[0041] Graphene oxide was ultrasonically dispersed in deionized water to obtain a 2 mg / mL suspension a, 3 g of chopped carbon fiber was added to 50 mL of suspension a, and after ultrasonic dispersion, the pH value was adjusted to 10 with sodium hydroxide to obtain a mixed solution b, two electrodes were inserted into the mixed solution b and the distance between the two was adjusted to 1 cm, and the mixture was operated at a constant voltage of 30 V for 1 hour. Finally, the composite staple fibers were separated and dried by a centrifuge.

[0042] Comparative Example 1

[0043] The comparative example is polyurethane type chopped carbon fiber (2 mm), which was purchased from Toray Industries, Ltd. of Japan. Example 3

[0044] The steps for preparing the functional components are as follows:

[0045] Step S1, adding 1.1g of tri(3-aminophenyl)phosphine oxide, 2.2g of fluorine-containing carbon branched dicarboxylic acid, 20mL of N-methylpyrrolidone and 5mL of pyridine into a flask, protecting with nitrogen, stirring at room temperature for 5min, adding 5mL of triphenyl phosphite, reacting at 20°C for 2h, then heating to 70°C for 2h, and finally heating to 130°C for 8h. After the reaction is completed, the reaction solution is precipitated and filtered in water, washed, and dried to obtain a hyperbranched polyamide;

[0046] Step S2, adding 10 g of hyperbranched polyamide and 100 mL of anhydrous methanol into a flask, stirring and then dropping a solution consisting of 1 g of 3,4-dihydroxybenzaldehyde and 20 mL of anhydrous methanol into the flask, and after the dropwise addition, reacting at 60° C. for 6 h under nitrogen protection, after the reaction is completed, pouring the reaction product into ice water, filtering, washing the filter cake with distilled water and drying to obtain a Schiff base hyperbranched polyamide;

[0047] Step S3, add 10g of Schiff base hyperbranched polyamide, 0.5g of potassium hydroxide and 100mL of anhydrous ethanol into a flask, stir and dissolve, then add 9.2g of epichlorohydrin, react at 70°C for 4h under nitrogen protection, cool to room temperature, add 5.6g of 40wt% potassium hydroxide aqueous solution dropwise, after the addition is complete, stir and react at 60°C for 6h, then cool to room temperature, filter, and evaporate the filtrate to remove anhydrous ethanol and water to obtain a functional component.

[0048] The preparation steps of fluorine-containing carbon branched dicarboxylic acid are as follows:

[0049] Step A1, 0.11 mol of diallylamine, 0.01 mol of DMAP and 100 mL of DMF were added to a flask, mixed evenly and then 0.1 mol of perfluoroheptanoyl chloride was added dropwise. After the addition was completed, the mixture was stirred at 100° C. for 8 h. After the reaction was completed, DMF was removed by distillation under reduced pressure, the distillation product was washed with water, and the organic phase was dried to obtain an intermediate product;

[0050] Step A2: 4.44 g of the intermediate product, 1.8 g of thioglycolic acid, 0.04 g of benzoin dimethyl ether and 60 mL of DMF were added to a flask, stirred and placed under an ultraviolet lamp for reaction for 30 min, and DMF was removed by reduced pressure distillation to obtain a fluorine-containing carbon branched dicarboxylic acid. Example 4

[0051] The steps for preparing the functional components are as follows:

[0052] Step S1, adding 1.2g of tri(3-aminophenyl)phosphine oxide, 2.2g of fluorine-containing carbon branched dicarboxylic acid, 20mL of N-methylpyrrolidone and 5mL of pyridine into a flask, protecting with nitrogen, stirring at room temperature for 10min, adding 5mL of triphenyl phosphite, reacting at 20°C for 2h, then heating to 70°C for 2h, and finally heating to 130°C for 8h. After the reaction is completed, the reaction solution is precipitated and filtered in water, washed, and dried to obtain a hyperbranched polyamide;

[0053] Step S2, adding 10 g of hyperbranched polyamide and 100 mL of anhydrous methanol into a flask, stirring and then dripping a solution consisting of 4 g of 3,4-dihydroxybenzaldehyde and 40 mL of anhydrous methanol into the flask, and after the dripping is completed, reacting at 60° C. for 6 h under nitrogen protection. After the reaction is completed, pouring the reaction product into ice water, filtering, washing the filter cake with distilled water and drying to obtain a Schiff base hyperbranched polyamide;

[0054] Step S3, add 10g of Schiff base hyperbranched polyamide, 0.5g of potassium hydroxide and 100mL of anhydrous ethanol into a flask, stir and dissolve, then add 9.2g of epichlorohydrin, react at 70°C for 4h under nitrogen protection, cool to room temperature, add 8.4g of 40wt% potassium hydroxide aqueous solution dropwise, after the addition is complete, stir and react at 60°C for 6h, then cool to room temperature, filter, and evaporate the filtrate to remove anhydrous ethanol and water to obtain a functional component.

[0055] The preparation steps of fluorine-containing carbon branched dicarboxylic acid are as follows:

[0056] Step A1, 0.12 mol of diallylamine, 0.01 mol of DMAP and 150 mL of DMF were added into a flask, mixed evenly and then 0.1 mol of perfluoroheptanoyl chloride was added dropwise. After the addition was completed, the mixture was stirred at 100° C. for 10 h. After the reaction was completed, DMF was removed by distillation under reduced pressure, the distillation product was washed with water, and the organic phase was dried to obtain an intermediate product;

[0057] Step A2: 4.44 g of the intermediate product, 2.0 g of thioglycolic acid, 0.06 g of benzoin dimethyl ether and 80 mL of DMF were added to a flask, stirred and placed under an ultraviolet lamp for reaction for 30 min, and DMF was removed by reduced pressure distillation to obtain a fluorine-containing carbon branched dicarboxylic acid.

[0058] Comparative Example 2

[0059] This comparative example is a Schiff base hyperbranched polyamide, specifically the product obtained in step S2 of Example 3.

[0060] Comparative Example 3

[0061] The steps for preparing the functional components are as follows:

[0062] Compared with Example 3, the "2.2 g of fluorine-containing carbon branched dicarboxylic acid" in step S1 of Example 3 is replaced by "0.54 g of adipic acid", and the remaining raw materials and preparation process are the same as in Example 3. Example 5

[0063] A composite staple fiber reinforced composite material comprises the following raw materials in parts by weight: 60 parts of nylon 6, 15 parts of the composite staple fibers of Example 1, 3 parts of the functional components of Example 3, 0.2 parts of a lubricant and 0.4 parts of an antioxidant.

[0064] The method for preparing the composite short fiber reinforced composite material comprises the following steps:

[0065] The raw materials are weighed according to the weight ratio, nylon 6, functional components, lubricants and antioxidants are put into a high-speed mixer and mixed for 3 minutes to obtain component one, and component one is fed into a twin-screw extruder through a main feeder, and composite staple fibers are added to the side feeder of the twin-screw extruder, and the mixture is subjected to extrusion, cooling, pelletizing and drying.

[0066] The speed of the twin-screw extruder is 300 rpm, the temperature is 220-280° C., the lubricant is stearic acid amide, and the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a ratio of 1:2. Example 6

[0067] A composite staple fiber reinforced composite material comprises the following raw materials in parts by weight: 65 parts of nylon 6, 20 parts of the composite staple fiber of Example 1, 5 parts of the functional component of Example 4, 0.5 parts of a lubricant and 0.6 parts of an antioxidant.

[0068] The method for preparing the composite short fiber reinforced composite material comprises the following steps:

[0069] The raw materials are weighed according to the weight ratio, nylon 6, functional components, lubricants and antioxidants are put into a high-speed mixer and mixed for 4 minutes to obtain component one, and component one is fed into a twin-screw extruder through a main feeder, and composite staple fibers are added to the side feeder of the twin-screw extruder, and the mixture is subjected to extrusion, cooling, pelletizing and drying.

[0070] Wherein, the speed of the twin-screw extruder is 350 rpm, the temperature is 220-280° C., the lubricant is polyethylene wax, and the antioxidant is the same as that in Example 5. Example 7

[0071] A composite staple fiber reinforced composite material comprises the following raw materials in parts by weight: 70 parts of nylon 6, 30 parts of composite staple fibers of Example 2, 7 parts of functional components of Example 4, 1 part of lubricant and 1 part of antioxidant.

[0072] The method for preparing the composite short fiber reinforced composite material comprises the following steps:

[0073] The raw materials are weighed according to the weight ratio, nylon 6, functional components, lubricants and antioxidants are put into a high-speed mixer and mixed for 5 minutes to obtain component one, and component one is fed into a twin-screw extruder through a main feeder, and composite staple fibers are added to the side feeder of the twin-screw extruder, and the mixture is subjected to extrusion, cooling, pelletizing and drying.

[0074] The speed of the twin-screw extruder is 400 rpm, the temperature is 220-280° C., the lubricant is paraffin, and the antioxidant is the same as that in Example 5.

[0075] Comparative Example 4

[0076] A composite staple fiber reinforced composite material. Compared with Example 5, the composite staple fibers in Example 5 are replaced with the materials in Comparative Example 1, and the remaining raw materials and preparation process are the same as those in Example 5.

[0077] Comparative Example 5

[0078] A composite short fiber reinforced composite material, compared with Example 5, the functional components in Example 5 are replaced with the substances in Comparative Example 2, and the remaining raw materials and preparation process are the same as Example 5.

[0079] Comparative Example 6

[0080] A composite short fiber reinforced composite material, compared with Example 5, the functional components in Example 5 are replaced with the product prepared in Comparative Example 3, and the remaining raw materials and preparation process are the same as Example 5.

[0081] The performance tests were performed on the composite short fiber reinforced composite materials obtained from Examples 5 to 7 and Comparative Examples 4 to 6. The tensile performance test was performed according to ISO527-2, the sample size was 150*10*4mm, and the tensile speed was 50mm / min; the simply supported beam impact strength was tested according to ISO179, and the sample size was 55*6*4; the melt flow index was tested according to ISO 1183 using the ISO test standard, and the water absorption of the composite material was tested according to GB / T 1034-2008 "Determination of Water Absorption of Plastics". According to GB2406-1993 standard, a limiting oxygen index tester was used, and the top ignition method was used to determine the blending

[0082] The limiting oxygen index of the sample strip, the sample length is about 100mm, the width is about 10mm, and the thickness is about 4mm. The test results are shown in Table 1:

[0083] Table 1

[0084] ;

[0085] It can be seen from the data recorded in Table 1 that, compared with Comparative Examples 3-5, the composite materials prepared in Examples 5-7 not only have good processing properties and mechanical properties, but also have good flame retardancy and water resistance.

[0086] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0087] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A composite short fiber reinforced composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 60-70 parts of nylon 6, 15-30 parts of composite staple fibers, 3-7 parts of functional components, 0.2-1 parts of lubricants and 0.4-1 parts of antioxidants; The composite short fibers are graphene oxide grafted short chopped carbon fibers; The steps for preparing the functional components are as follows: Step S1, tri(3-aminophenyl)phosphine oxide, fluorine-containing carbon branched dicarboxylic acid, N-methylpyrrolidone and pyridine are mixed, nitrogen protection is applied, triphenyl phosphite is added after stirring, and the mixture is reacted at 20° C. for 2 h, then at 70° C. for 2 h, and then at 130° C. for 8 h to obtain a hyperbranched polyamide; Step S2, mixing the hyperbranched polyamide and anhydrous methanol, adding dropwise the 3,4-dihydroxybenzaldehyde methanol solution, and after the dropwise addition is completed, reacting at 60° C. for 6 h under nitrogen protection to obtain a Schiff base hyperbranched polyamide; Step S3, mixing Schiff base hyperbranched polyamide, potassium hydroxide and anhydrous ethanol, adding epichlorohydrin, reacting at 70° C. for 4 h under nitrogen protection, cooling to room temperature, dropping potassium hydroxide aqueous solution, after the dropwise addition is complete, stirring at 60° C. for 6 h and then cooling to room temperature to obtain a functional component; In step S1, the amount ratio of tris(3-aminophenyl)phosphine oxide, fluorine-containing carbon branched dicarboxylic acid, N-methylpyrrolidone, pyridine and triphenyl phosphite is 1.1-1.2 g: 2.2 g: 20 mL: 5 mL: 5 mL; In step S2, the mass ratio of the hyperbranched polyamide to 3,4-dihydroxybenzaldehyde is 10:1-4; In step S3, the amount ratio of Schiff base hyperbranched polyamide, potassium hydroxide, anhydrous ethanol, epichlorohydrin and potassium hydroxide aqueous solution is 10g:0.5g:100mL:9.2g:5.6-8.4g, and the mass fraction of potassium hydroxide aqueous solution is 40%; The steps for preparing composite staple fibers are as follows: Graphene oxide is ultrasonically dispersed in deionized water to obtain a suspension a, short-cut carbon fibers are added to the suspension a, and after being uniformly ultrasonically dispersed, the pH value is adjusted to 10 with sodium hydroxide to obtain a mixed solution b, two electrodes are inserted into the mixed solution b and the distance between the two is adjusted to 1 cm, and the mixture is operated at a constant voltage of 30 V for 1 hour, and finally separated and dried by a centrifuge to obtain composite short fibers; The concentration of graphene oxide in suspension a is 2 mg / mL, the amount ratio of suspension a to chopped carbon fiber is 30-50 mL: 3 g, and the chopped carbon fiber is high-carbon glue-free carbon fiber chopped strands.

2. The method for preparing a composite short fiber reinforced composite material according to claim 1, characterized in that: The following steps are involved: Weigh the raw materials according to the weight ratio, put nylon 6, functional components, lubricants and antioxidants into a high-speed mixer and mix for 3-5 minutes to obtain component one, feed component one into a twin-screw extruder through a main feeder, add composite staple fibers into the side feeder of the twin-screw extruder, and perform extrusion, cooling, pelletizing and drying.