Negative electrode material and preparation method thereof, and battery
By preparing a negative electrode material with secondary particles dispersed with carbon material and silicon grains, the problems of poor electrochemical performance and low cycle stability caused by volume expansion of silicon negative electrode material are solved, and low expansion, high cycle stability and High rate performance.
Patent Information
- Application Number
- CN202311778680.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-12-21
AI Technical Summary
The silicon negative electrode material is difficult to commercially use due to large volume expansion in lithium-ion batteries.
By preparing a negative electrode material with secondary particles dispersed with carbon material and silicon grains, the crystallization instability is controlled, and the vapor phase carbon deposition and coating material are used to form a silicon-carbon composite material with low expansion and high cycle stability.
The conductivity and structural stability of the negative electrode material are improved, the expansion rate is reduced, the circulation and rate performance are enhanced, and the first-time Coulomb efficiency is achieved.
Smart Images

Figure CN117913231B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials, and in particular to negative electrode materials and preparation methods thereof, and batteries. Background Art
[0002] Lithium-ion batteries are widely used in electric vehicles and consumer electronics due to their advantages such as high energy density, high output power, long cycle life and low environmental pollution.
[0003] In order to improve the energy density of batteries, the research and development of silicon negative electrode materials are becoming more mature. However, the volume expansion of silicon negative electrode materials is large (>300%) during the process of lithium extraction and insertion. Silicon negative electrode materials will pulverize and fall from the current collector during the charging and discharging process, causing the silicon particles to lose electrical contact with the current collector, resulting in poor electrochemical performance, capacity attenuation, and decreased cycle stability, making it difficult to obtain commercial applications. In order to improve the conductivity and cycle stability of silicon negative electrode materials, carbon coating can be used. The existing carbon coating preparation method has complicated steps, and simple carbon coating cannot effectively improve the electrochemical performance of silicon-carbon negative electrodes.
[0004] Based on this, there is an urgent need to develop a silicon-carbon negative electrode material with long cycle and low expansion. Summary of the invention
[0005] The present application proposes a negative electrode material and a preparation method thereof, and a battery, so that the negative electrode material has high initial efficiency, excellent cycle stability and low expansion performance.
[0006] In a first aspect, the present application provides a negative electrode material, the negative electrode material comprising secondary particles, the secondary particles comprising carbon material and primary particles, the primary particles comprising at least one silicon grain;
[0007] The average particle size of silicon crystals of the negative electrode material measured at 25°C is M0 nm; the average particle size of silicon crystals of the negative electrode material measured at 25°C after being heated to 1000°C under nitrogen protection and kept warm for 1 hour and then naturally cooled to 25°C is M1 nm;
[0008] The crystal instability of the negative electrode material is F, where F=(M1-M0) / M0, M1>M0, and 0.01≤F≤500.
[0009] In some embodiments, the average particle size of the primary particles is 1 nm to 100 nm.
[0010] In some embodiments, the pore volume of the negative electrode material is 0.01 cm 3 / g~0.2cm 3 / g.
[0011] In some embodiments, the negative electrode material is heated to 1000° C. at a heating rate of 5° C. / min under nitrogen protection, kept at that temperature for 1 hour, and then naturally cooled to 25° C. The average particle size of silicon grains measured is M1 nm, 0.1<M1≤50;
[0012] In some embodiments, the average particle size of silicon grains of the negative electrode material measured at 25° C. is M0 nm, and 0.1≤M0≤20.
[0013] In some embodiments, the mass content of oxygen in the negative electrode material is less than 15%.
[0014] In some embodiments, the mass content of silicon in the negative electrode material is 40% to 80%.
[0015] In some embodiments, the carbon material includes at least one of amorphous carbon and graphitized carbon.
[0016] In some embodiments, the negative electrode material further includes a coating material located on at least a portion of the surface of the secondary particles.
[0017] In some embodiments, the coating material includes at least one of an amorphous carbon material, a graphitized carbon material, and a polymer.
[0018] In some embodiments, the coating material includes a polymer, and the polymer includes at least one of polyacrylic acid, polyacrylonitrile, polyimide, polyurethane, polydopamine, xanthan gum, polypyrrole, polythiophene, polyphenylene vinylene, polyaniline, polyacetylene, and tannic acid.
[0019] In some embodiments, the coating material includes a polymer, and the coating layer formed by the coating material has a thickness of 50 nm to 300 nm.
[0020] In some embodiments, the coating material includes a graphitized carbon material, and the coating layer formed by the coating material has a thickness of 5 nm to 100 nm.
[0021] In some embodiments, the coating material includes an amorphous carbon material, and the coating layer formed by the coating material has a thickness of 10 nm to 500 nm.
[0022] In some embodiments, the mass content of carbon in the negative electrode material is 5% to 80%.
[0023] In some embodiments, the tap density of the negative electrode material is 0.3 g / cm 3 ~1.3g / cm 3 .
[0024] In some embodiments, the powder compaction density of the negative electrode material is 1.2 g / cm 3 ~1.8g / cm 3 .
[0025] In some embodiments, the median particle size of the negative electrode material is 0.5 μm to 26 μm.
[0026] In some embodiments, the specific surface area of the negative electrode material is 0.8 m 2 / g~40m 2 / g.
[0027] In a second aspect, the present application provides a method for preparing a negative electrode material, comprising the following steps:
[0028] The mixture containing silicon element powder and silicon micropowder is subjected to a sintering treatment to obtain an intermediate;
[0029] The intermediate is subjected to secondary sintering treatment, so that the intermediate undergoes a disproportionation reaction to obtain a precursor;
[0030] Placing the precursor in an etching solution for etching to obtain silicon particles with holes;
[0031] The silicon particles having pores are subjected to vapor phase carbon deposition using a first vapor phase carbon source to obtain secondary particles, and the negative electrode material includes the secondary particles.
[0032] In some embodiments, the mass content of oxygen in the silicon powder is ≤5%.
[0033] In some embodiments, the molar ratio of the silicon element powder to the silicon fine powder is 1:(0.9-1.1).
[0034] In some embodiments, the primary sintering process is performed at a temperature of 1150°C to 1650°C.
[0035] In some embodiments, the time of the primary sintering treatment is 3 hours to 12 hours.
[0036] In some embodiments, the heating rate of the primary sintering process is 1° C. / min to 20° C. / min.
[0037] In some embodiments, the pressure of the primary sintering process is ≤10Pa.
[0038] In some embodiments, the secondary sintering process is performed at a temperature of 200°C to 1050°C.
[0039] In some embodiments, the secondary sintering treatment lasts for 1 hour to 48 hours.
[0040] In some embodiments, the heating rate of the secondary sintering process is 1° C. / min to 30° C. / min.
[0041] In some embodiments, the mass ratio of the precursor to the etching solution is 1:(5-20).
[0042] In some embodiments, the etching solution includes hydrofluoric acid, water, ethanol and ammonium fluoride;
[0043] In some embodiments, the etching solution includes hydrofluoric acid, water, ethanol and ammonium fluoride, wherein the mass ratio of the hydrofluoric acid, the water, the ethanol and the ammonium fluoride is (6-24):3:1:(3-6);
[0044] In some embodiments, the etching solution includes hydrofluoric acid, water, ethanol and ammonium fluoride, wherein the mass concentration of the hydrofluoric acid is 40%;
[0045] In some embodiments, the etching reaction time is 0.5 h to 10 h.
[0046] In some embodiments, the temperature of the etching reaction is ≤ 40°C.
[0047] In some embodiments, the method further comprises washing and drying the etching reaction product.
[0048] In some embodiments, the mass content of oxygen in the silicon particles having pores is less than 5%.
[0049] In some embodiments, the mass content of water in the silicon particles having pores is less than 1%.
[0050] In some embodiments, the heating rate of the vapor phase carbon deposition is 1° C. / min to 30° C. / min.
[0051] In some embodiments, the reaction temperature of the vapor phase carbon deposition is 200°C to 1050°C.
[0052] In some embodiments, the holding time of the vapor phase carbon deposition is 1 hour to 48 hours.
[0053] In some embodiments, the first gas-phase carbon source includes at least one of acetylene, methane, ethylene, propane, toluene, cyclohexane, ethanol, ethylene, propylene, pyrrole, and acetonitrile.
[0054] In some embodiments, the flow rate of the first gas-phase carbon source is 0.1 L / min to 10 L / min.
[0055] In some embodiments, the method further comprises: performing surface coating treatment on the secondary particles using a coating material.
[0056] In some embodiments, the coating material includes at least one of an amorphous carbon material, a graphitized carbon material, and a polymer.
[0057] In some embodiments, the step of coating the secondary particles with a coating material comprises: spray-drying a mixed coating liquid containing the secondary particles and a polymer.
[0058] In some embodiments, the step of coating the surface of the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the solid content of the secondary particles in the mixed coating liquid is 5% to 50%.
[0059] In some embodiments, the mixed coating solution includes a polar solvent.
[0060] In some embodiments, the polar solvent includes at least one of water, anhydrous ethanol, methanol and isopropanol.
[0061] In some embodiments, the mass ratio of the secondary particles to the polymer is 10:(0.1-5).
[0062] In some embodiments, the drying temperature of the spray drying is 60°C to 200°C.
[0063] In some embodiments, the polymer includes at least one of polyacrylic acid, polyacrylonitrile, polyimide, polyurethane, polydopamine, xanthan gum, polypyrrole, polythiophene, polyphenylene vinylene, polyaniline, polyacetylene and tannic acid;
[0064] In some embodiments, the step of coating the secondary particles with a coating material comprises: introducing a second gas-phase carbon source into the secondary particles, heating the second gas-phase carbon source until a thermal cracking reaction occurs, so that the coating material is deposited on the surface of the secondary particles, and the coating material comprises at least one of an amorphous carbon material and a graphitized carbon material;
[0065] In some embodiments, the gas-phase carbon source includes at least one of acetylene, methane, toluene, cyclohexane, ethanol, ethylene, and propylene.
[0066] In some embodiments, the concentration of the gaseous carbon source is 0.1 L / min to 10 L / min;
[0067] In some embodiments, the temperature of the thermal cracking reaction is 600° C. to 1000° C., and the insulation time is 1 h to 48 h.
[0068] In a third aspect, the present application provides a battery, comprising the negative electrode material or the negative electrode material prepared by the method for preparing the negative electrode material.
[0069] The technical solution of this application has at least the following beneficial effects:
[0070] First, the negative electrode material provided by the present application includes secondary particles, the secondary particles include mutually dispersed carbon materials and primary particles, and the primary particles include at least one silicon grain; the present application controls the crystallization instability of the negative electrode material to F, 0.01≤F≤500, so as to reduce the grain boundary surface energy of the primary particles, weaken the stress concentration phenomenon generated by the primary particles during the lithium insertion and deintercalation process, improve the electrochemical sintering phenomenon of the negative electrode material after lithium insertion, improve the structural stability of the primary particles during the lithiation process, reduce the expansion rate of the negative electrode material, and facilitate the formation of a stable solid electrolyte film, thereby improving the electrochemical performance of the negative electrode material; in addition, in the secondary particles of the negative electrode material, the carbon material and the primary particles are mutually dispersed, which can effectively improve the conductivity of the primary particles and can also effectively alleviate the volume expansion of the primary particles; part of the carbon material is located on the surface of the secondary particles, which can further alleviate the volume expansion of the negative electrode material, and can also effectively reduce the side reaction of the primary particles with the electrolyte, while enhancing the structural stability of the negative electrode material, so that the negative electrode material has low expansion, high cycle stability, high rate and high first coulomb efficiency.
[0071] Secondly, the preparation method of the negative electrode material provided in the present application is to first sinter a mixture of silicon element powder and silicon micropowder so that the silicon element can undergo an oxidation-reduction reaction with silicon dioxide to form silicon monoxide, and then the silicon oxide is subjected to a secondary sintering treatment. At this time, the silicon monoxide undergoes a disproportionation reaction. Due to the presence of silicon dioxide, the growth of silicon grains can be limited, the size of the generated silicon grains can be reduced, the stress concentration generated during the lithiation of the primary particles can be weakened, the structural stability of the primary particles during the lithiation process can be improved, the expansion rate of the negative electrode material can be reduced, and it is conducive to the formation of a stable solid electrolyte membrane, thereby improving the electrochemical properties of the negative electrode material; then, by etching, excess silicon dioxide and other impurities are removed to form silicon particles with holes, and finally, gas phase carbon deposition is performed so that the carbon material can be deposited into the pores of the silicon particles and at least part of the surface of the silicon particles to obtain secondary particles. In the secondary particles of the negative electrode material, the carbon material and the primary particles are dispersed with each other, which can effectively improve the conductivity of the primary particles and effectively alleviate the volume expansion of the primary particles; part of the carbon material is located on the surface of the secondary particles, which can further alleviate the volume expansion of the negative electrode material, and can also effectively reduce the side reactions between the primary particles and the electrolyte, while enhancing the structural stability of the negative electrode material, so that the negative electrode material has low expansion, high cycle stability, high rate capability and high first coulombic efficiency.
[0072] The method for preparing the negative electrode material provided in the present application can not only improve the electrochemical properties of the material, but also be suitable for large-scale production. The prepared negative electrode material can effectively improve the rate performance and cycle stability of the lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] Figure 1 A schematic diagram of the structure of the negative electrode material provided in this embodiment;
[0074] Figure 2 A schematic diagram of a process for preparing a negative electrode material provided in this embodiment;
[0075] Figure 3 This is the XRD diagram of the silicon-carbon composite negative electrode material of Example 1;
[0076] Figure 4a and Figure 4b They are respectively a scanning electron microscope image and an internal cross-sectional view of the negative electrode material prepared in Example 1;
[0077] Figure 5a This is a transmission electron microscope image of the negative electrode material prepared in Example 1;
[0078] Figure 5b It is a partial enlarged transmission electron microscope image of the negative electrode material prepared in Example 1;
[0079] Figure 6 This is the cycle performance curve of the negative electrode material prepared in Example 1. DETAILED DESCRIPTION
[0080] The following is a preferred implementation of the embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the embodiment of the present invention. These improvements and modifications are also considered to be within the scope of protection of the embodiment of the present invention.
[0081] At present, in lithium-ion batteries, negative electrode materials are one of the key materials that affect their charge and discharge performance. In order to improve the energy density of batteries, the research and development of high-capacity negative electrode materials are becoming more and more mature. However, these negative electrode materials have a large volume expansion during the alloying process with lithium. The negative electrode materials will be pulverized and fall off the current collector during the charge and discharge process, causing the negative electrode materials to lose electrical contact with the current collector, resulting in poor electrochemical performance of the battery, capacity attenuation, and decreased cycle stability, making it difficult to obtain commercial applications.
[0082] During the lithium extraction process of silicon materials, there will be changes in macroscopic structure, mechanical state and interface effect, which are closely related to the grain size, primary particle size and constructed secondary particle size of silicon materials. At present, there is no suitable balance point for the size ratio of silicon grains, primary particles and secondary particles, which leads to stress concentration in silicon negative electrode materials during lithium extraction, easy particle rupture and poor structural stability of negative electrode materials.
[0083] In a first aspect, the present application provides a negative electrode material, such as Figure 1 As shown, the negative electrode material includes secondary particles 13, the secondary particles 13 include mutually dispersed carbon materials 12 and primary particles 11, and the primary particles 11 include at least one silicon grain;
[0084] The average particle size of silicon crystals of the negative electrode material measured at 25°C is M0 nm; the average particle size of silicon crystals of the negative electrode material measured at 25°C after being heated to 1000°C under nitrogen protection and kept warm for 1 hour and then naturally cooled to 25°C is M1 nm;
[0085] The crystal instability of the negative electrode material is F, where F=(M1-M0) / M0, M1>M0, and 0.01≤F≤500.
[0086] In the above scheme, the negative electrode material includes secondary particles, the secondary particles include mutually dispersed carbon materials and primary particles, and the primary particles include at least one silicon grain; the present application controls the crystallization instability of the negative electrode material to F, 0.01≤F≤500, which can reduce the grain boundary surface energy of the primary particles, weaken the stress concentration phenomenon generated by the primary particles during the lithium insertion and deintercalation process, improve the electrochemical sintering phenomenon of the negative electrode material after lithium insertion, improve the structural stability of the primary particles during the lithiation process, reduce the expansion rate of the negative electrode material, and is conducive to forming a stable solid electrolyte membrane, thereby improving the electrochemical performance of the negative electrode material; in addition, in the secondary particles of the negative electrode material, the carbon material and the primary particles are dispersed with each other, which can effectively improve the conductivity of the primary particles and can also effectively alleviate the volume expansion of the primary particles; part of the carbon material is located on the surface of the secondary particles, which can further alleviate the volume expansion of the negative electrode material, and can also effectively reduce the side reactions of the primary particles and the electrolyte, while enhancing the structural stability of the negative electrode material, so that the negative electrode material has low expansion, high cycle stability, high rate and high first coulomb efficiency.
[0087] In some embodiments, the average particle size of the primary particles 11 is 1 nm to 100 nm; specifically, it can be 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 30 nm, 40 nm, 50 nm, 80 nm or 100 nm, etc., which is not limited here.
[0088] In some embodiments, the average particle size of silicon grains of the negative electrode material measured at 25°C is M0 nm, 0.1≤M0≤20, and can be 0.1nm, 1nm, 3nm, 5nm, 8nm, 10nm, 12nm, 15nm, 18nm or 20nm, etc., which is not limited here.
[0089] In some embodiments, the average particle size of silicon grains measured when the negative electrode material is heated to 1000°C at a heating rate of 5°C / min under nitrogen protection and kept at that temperature for 1 hour and then naturally cooled to 25°C is M1 nm, 0.1<M1≤50; specifically, it can be 0.11nm, 1nm, 3nm, 5nm, 8nm, 10nm, 15nm, 20nm, 30nm, 35nm, 40nm, 45nm or 50nm, etc., which is not limited here. Preferably, 1≤M1≤30.
[0090] In some embodiments, the crystal instability of the negative electrode material is F, F = (M1-M0) / M0, 0.01≤F≤500, specifically 0.01, 0.2, 0.5, 1, 5, 10, 20, 50, 80, 100, 200, 300, 400 or 500, etc., of course, it can also be other values within the above range, which are not limited here. The crystal instability of silicon in the negative electrode material affects the stability of the structure of the entire negative electrode material after lithiation. The smaller the crystal instability value of the negative electrode material, the more difficult it is for the grains of the negative electrode material to grow at high temperatures, the larger the grain boundary energy of the silicon in the negative electrode material, the less likely the primary particles are to undergo electrochemical sintering during the lithiation process, and the stress concentration generated is effectively suppressed, the structural stability of the negative electrode material is ensured, the expansion rate of the negative electrode material is reduced, and it is conducive to the formation of a stable solid electrolyte membrane, thereby improving the electrochemical performance and cycle performance of the negative electrode material.
[0091] In some embodiments, the carbon material 12 includes at least one of amorphous carbon and graphitized carbon. The primary particles 11 are dispersed in the carbon material 12 , which can improve the conductivity of the primary particles 11 and effectively alleviate the volume expansion of the primary particles 11 .
[0092] In some embodiments, the negative electrode material further includes a coating material 121 located on at least a portion of the surface of the secondary particles 13 , and the coating material includes at least one of an amorphous carbon material, a graphitized carbon material, and a polymer.
[0093] In some embodiments, the coating material is located on the surface of the secondary particles to form a coating layer, and the thickness of the coating layer is 5 nm to 500 nm.
[0094] It can be understood that constructing a coating layer on the surface of the secondary particles can further alleviate the volume expansion of the negative electrode material; using the coating layer to synergistically modify the secondary particles can effectively alleviate the volume expansion of the primary particles, ensuring that the negative electrode material still has excellent electrical contact performance after lithium insertion. The coating layer can also effectively reduce the side reactions between the primary particles and the electrolyte, while enhancing the structural stability of the negative electrode material.
[0095] In some embodiments, the coating material includes a polymer, and illustratively, the polymer may be at least one of a diblock copolymer, a triblock copolymer, and a multiblock copolymer.
[0096] In some embodiments, the coating material includes a polymer, and the thickness of the coating layer formed by the coating material is 50nm to 300nm, specifically 50nm, 80nm, 100nm, 150nm, 200nm, 250nm or 300nm, etc., which is not limited here.
[0097] In some embodiments, the polymer includes at least one of polyacrylic acid, polyacrylonitrile, polyimide, polyurethane, polydopamine, xanthan gum, polypyrrole, polythiophene, polyphenylene vinylene, polyaniline, polyacetylene and tannic acid. The polymer is preferably at least one of polypyrrole, polythiophene, polyaniline, polyaniline and polyacetylene.
[0098] In some embodiments, the coating material includes a graphitized carbon material, and the thickness of the coating layer formed by the coating material is 5nm to 100nm, specifically 5nm, 10nm, 30nm, 50nm, 70nm, 80nm, 90nm or 100nm, etc., which is not limited here.
[0099] In some embodiments, the coating material includes an amorphous carbon material, and the thickness of the coating layer formed by the coating material is 10nm to 500nm; specifically, it can be 10nm, 50nm, 80nm, 100nm, 150nm, 200nm, 250nm, 300nm, 450nm or 500nm, etc., which is not limited here.
[0100] In some embodiments, the pore volume of the negative electrode material is 0.01 cm 3 / g~0.2cm 3 / g, specifically 0.01cm 3 / g, 0.03cm 3 / g, 0.05cm 3 / g, 0.08cm 3 / g, 0.1cm 3 / g, 0.13cm 3 / g, 0.15cm 3 / g, 0.18cm 3 / g or 0.2cm 3 / g, etc., are not limited here.
[0101] In some embodiments, the tap density of the negative electrode material is 0.3 g / cm 3 ~1.3g / cm 3 , specifically 0.3g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 , 1.0g / cm 3 , 1.3g / cm 3 The tap density of the negative electrode material is preferably 0.6 g / cm 3 ~0.9g / cm 3 .
[0102] In some embodiments, the powder compaction density of the negative electrode material is 1.2 g / cm 3 ~1.8g / cm 3 , for example 1.2 g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 or 1.8 g / cm 3 The compacted density of the negative electrode material is preferably 1.45 g / cm 3 ~1.75g / cm 3 .
[0103] In some embodiments, the median particle size of the negative electrode material is 0.5 μm to 26 μm. Optionally, the median particle size of the negative electrode material can be 0.5 μm, 1 μm, 3 μm, 4 μm, 5 μm, 7 μm, 10 μm, 13 μm, 15 μm, 20 μm or 26 μm, etc., which are not limited here. The median particle size of the negative electrode material is preferably 1 μm to 10 μm, and more preferably 3 μm to 7 μm.
[0104] The specific surface area ratio of the negative electrode material is 0.8m 2 / g~40m 2 Optionally, the specific surface area ratio of the negative electrode material can be 0.8m 2 / g, 1m 2 / g, 5m 2 / g, 8m 2 / g, 10m 2 / g, 15m 2 / g, 20m2 / g, 25m 2 / g, 30m 2 / g, 35m 2 / g or 40m 2 / g, etc., which are not limited here; it can be understood that too large specific surface area is easy to lead to the formation of SEI film, consume too much irreversible lithium salt, and reduce the initial efficiency of the battery. Considering the cost of the preparation process, the specific surface area is controlled within 1m 2 / g~20m 2 / g.
[0105] In some embodiments, the mass content of carbon in the negative electrode material is 5% to 80%. Specifically, it can be 5%, 8%, 10%, 15%, 20%, 30%, 35%, 40%, 45%, 50%, 60%, 70% or 80%, etc., which is not limited here. It should be noted that the carbon in the negative electrode material comes from the carbon material.
[0106] In some embodiments, the mass content of oxygen in the negative electrode material is less than 15%, and may be 5%, 6%, 8%, 10%, 12%, 13%, 14% or 14.9%, etc., which is not limited here.
[0107] In some embodiments, the mass content of silicon in the negative electrode material is 40% to 80%, specifically 40%, 42%, 45%, 48%, 50%, 55%, 60%, 65%, 68%, 70% or 80%, etc., which is not limited here.
[0108] The present application also provides a method for preparing a negative electrode material, such as Figure 2 As shown, the method includes the following steps S10 to S40:
[0109] S10, sintering the mixture containing silicon element powder and silicon micropowder to obtain an intermediate;
[0110] S20, performing a secondary sintering treatment on the intermediate so that the intermediate undergoes a disproportionation reaction to obtain a precursor;
[0111] S30, placing the precursor in an etching solution for etching to obtain silicon particles with holes;
[0112] S40, performing vapor phase carbon deposition on silicon particles having pores using a first vapor phase carbon source to obtain secondary particles, wherein the negative electrode material includes the secondary particles.
[0113] Secondly, the preparation method of the negative electrode material provided in the present application is to first sinter a mixture of silicon element powder and silicon micropowder so that the silicon element can undergo a reduction reaction with silicon dioxide to form silicon monoxide, and then the silicon oxide is subjected to a secondary sintering treatment. At this time, the silicon monoxide undergoes a disproportionation reaction. Due to the presence of silicon dioxide, the growth of silicon grains can be limited, the size of the generated silicon grains can be reduced, the stress concentration generated during the lithiation of the primary particles can be weakened, the structural stability of the primary particles during the lithiation process can be improved, the expansion rate of the negative electrode material can be reduced, and it is conducive to the formation of a stable solid electrolyte membrane, thereby improving the electrochemical properties of the negative electrode material; then, by etching, excess silicon dioxide and other impurities are removed to form silicon particles with holes, and finally, gas phase carbon deposition is performed so that the carbon material can be deposited into the pores of the silicon particles and at least part of the surface of the silicon particles to obtain secondary particles. In the secondary particles of the negative electrode material, the carbon material and the primary particles are dispersed with each other, which can effectively improve the conductivity of the primary particles and effectively alleviate the volume expansion of the primary particles; part of the carbon material is located on the surface of the secondary particles, which can further alleviate the volume expansion of the negative electrode material, and can also effectively reduce the side reactions between the primary particles and the electrolyte, while enhancing the structural stability of the negative electrode material, so that the negative electrode material has low expansion, high cycle stability, high rate capability and high first coulombic efficiency.
[0114] The method for preparing the negative electrode material provided in the present application can not only improve the electrochemical properties of the material, but also be suitable for large-scale production. The prepared negative electrode material can effectively improve the rate performance and cycle stability of the lithium battery.
[0115] The preparation method of the present application is described in detail below with reference to the examples:
[0116] Step S10, sintering the mixture containing silicon element powder and silicon micropowder to obtain an intermediate.
[0117] In some embodiments, the mass content of oxygen in the silicon micropowder is ≤5%, and can be specifically 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5% or 1%, etc., and can certainly be other values within the above range, which is not limited here.
[0118] In some embodiments, the molar ratio of silicon element powder to silicon micropowder is 1:(0.9-1.1), specifically 1:0.9, 1:0.95, 1:1.0, 1:1.05, 1:1.08, 1:1.09 or 1.1, etc., and of course it can also be other values within the above range, which is not limited here.
[0119] In some embodiments, step S10 may specifically include placing a mixture of silicon elemental powder and silicon micropowder into a vacuum reaction chamber, evacuating the vacuum reaction chamber to a pressure of ≤10 Pa, and then performing a sintering process.
[0120] In some embodiments, the temperature of a sintering treatment is 1150°C to 1650°C, specifically 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, 1550°C, 1600°C or 1650°C, etc., and of course it can also be other values within the above range, which is not limited here.
[0121] In some embodiments, the time for a sintering treatment is 3 h to 12 h, specifically 3 h, 4 h, 6 h, 8 h, 9 h, 10 h or 12 h, etc., and of course, it can also be other values within the above range, which is not limited here.
[0122] In some embodiments, the heating rate of a single sintering treatment is 1°C / min to 20°C / min, specifically 1°C / min, 3°C / min, 5°C / min, 8°C / min, 10°C / min, 15°C / min or 20°C / min, etc. Of course, it can also be other values within the above range, which is not limited here.
[0123] In some embodiments, the pressure of a sintering process is ≤10Pa, and may be specifically 10Pa, 9Pa, 8Pa, 7Pa, Pa, 5Pa, 3Pa, 2Pa or 1Pa, etc., and may be other values within the above range, which is not limited here.
[0124] Step S20, performing a secondary sintering process on the intermediate so that the intermediate undergoes a disproportionation reaction to obtain a precursor.
[0125] In some embodiments, the temperature of the secondary sintering treatment is 200°C to 1050°C, specifically 200°C, 300°C, 400°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 890°C, 900°C, 980°C or 1050°C, etc., and of course it can also be other values within the above range, which is not limited here.
[0126] In some embodiments, the time of the secondary sintering treatment is 1 h to 48 h, specifically 1 h, 2 h, 4 h, 6 h, 8 h, 10 h, 15 h, 20 h, 24 h, 30 h, 36 h, 42 h or 48 h, etc., and of course it can also be other values within the above range, which is not limited here.
[0127] In some embodiments, the heating rate of the secondary sintering treatment is 1°C / min to 30°C / min, specifically 1°C / min, 3°C / min, 5°C / min, 8°C / min, 10°C / min, 15°C / min, 20°C / min, 25°C / min or 30°C / min, which is not limited here.
[0128] In the present application, by controlling the temperature, time and heating rate of the secondary sintering treatment, part of the intermediates can undergo a disproportionation reaction. The general reaction formula is: 2SiO=Si+SiO2. Since the generated silicon dioxide limits the growth of silicon grains, small-sized silicon grains can be dispersed in the precursor, and then after subsequent etching treatment, silicon particles with holes can be formed.
[0129] Step S30, placing the precursor in an etching solution for etching to obtain silicon particles with holes.
[0130] In some embodiments, the mass ratio of the precursor to the etching solution is 1:(5-20), specifically 1:5, 1:8, 1:10, 1:12, 1:15, 1:18 or 1:20, etc. Of course, it can also be other values within the above range, which is not limited here.
[0131] In some embodiments, the etching solution comprises hydrofluoric acid, water, ethanol, and ammonium fluoride, and the mass ratio of hydrofluoric acid, water, ethanol, and ammonium fluoride is (6-24):3:1:(3-6), and specifically can be 6:3:1:3, 10:3:1:3, 12:3:1:3, 15:3:1:3, 18:3:1:3, 20:3:1:3, 24:3:1:3, 6:3:1:5, 6:3:1:6, etc., and of course, it can also be other values within the above range, which are not limited here. It can be understood that the addition of ammonium fluoride can control the reaction rate, reduce the oxidation of silicon particles caused by local heat release, reduce the formation of inactive silicon dioxide, and improve the specific capacity of the negative electrode material.
[0132] In some embodiments, the mass concentration of hydrofluoric acid is 37% to 50%, specifically 37%, 39%, 40%, 42%, 45%, 46%, 48% or 50%, etc., and may be other values within the above range, which is not limited here.
[0133] In some embodiments, the etching reaction time is 0.5 h to 10 h, and specifically can be 0.1 h, 1 h, 2 h, 4 h, 6 h, 8 h, 9 h or 10 h, which is not limited here.
[0134] In some embodiments, the temperature of the etching reaction is ≤40°C, and can be 40°C, 38°C, 36°C, 35°C, 32°C, 30°C, 28°C, 25°C, 20°C or 15°C, etc., and can also be other values within the above range, which is not limited here.
[0135] In some embodiments, the method further comprises washing and drying the etching reaction product.
[0136] In some embodiments, the mass content of oxygen in the silicon particles with holes is less than 5%, and can be 4.9%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5% or 1%, etc., and can be other values within the above range, which is not limited here.
[0137] In some embodiments, the mass content of water in the silicon particles with holes is less than 1%, and can be specifically 0.99%, 0.9%, 0.8%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2% or 0.1%, etc., and of course can also be other values within the above range, which is not limited here.
[0138] Step S40 , using a first gas-phase carbon source to perform gas-phase carbon deposition on silicon particles having pores to obtain a negative electrode material.
[0139] It can be understood that during the gas-phase carbon deposition process, the first gas-phase carbon source enters the pores of the silicon particles and is deposited to form carbon materials, and part of the carbon materials is deposited on the surfaces of the silicon particles.
[0140] In some embodiments, the temperature of vapor phase carbon deposition is 200° C. to 1050° C., specifically, the reaction temperature may be 200° C., 300° C., 400° C., 500° C., 550° C., 600° C., 650° C., 700° C., 750° C., 800° C., 890° C., 900° C., 980° C., or 1050° C. Preferably, the reaction temperature is 700° C. to 900° C.
[0141] In some embodiments, the holding time of the vapor phase carbon deposition is 1 h-48 h, and specifically can be 1 h, 4 h, 8 h, 12 h, 16 h, 24 h, 28 h, 32 h, 38 h or 48 h, which is not limited here.
[0142] In some embodiments, the first gas-phase carbon source includes at least one of acetylene, methane, ethylene, propane, toluene, cyclohexane, ethanol, ethylene, propylene, pyrrole, and acetonitrile.
[0143] In some embodiments, the flow rate of the first gas-phase carbon source is 0.1 L / min-10 L / min, specifically 0.1 L / min, 0.4 L / min, 0.6 L / min, 0.8 L / min, 1.0 L / min, 2 L / min, 5 L / min, 6 L / min, 8 L / min, 9 L / min or 10 L / min, etc., which is not limited here.
[0144] The present application can improve the reaction efficiency of vapor phase carbon deposition by controlling the time, temperature and holding time of vapor phase carbon deposition, so that carbon material is deposited in the pores of silicon particles. The carbon material deposited in the pores of silicon particles can improve the conductivity of the negative electrode material. The carbon material deposited on the surface of the silicon particles can also form a carbon layer, which can be an amorphous carbon material, thereby buffering the volume expansion of the silicon particles, reducing the direct contact between the silicon particles and the electrolyte, and improving the cycle performance of the negative electrode material.
[0145] After step S40, the method further includes: performing surface coating treatment on the secondary particles by using a coating material, wherein the coating material includes at least one of an amorphous carbon material, a graphitized carbon material, and a polymer.
[0146] In some embodiments, the step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer.
[0147] In some embodiments, the solid content of the secondary particles in the mixed coating liquid is 5% to 50%, specifically 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc., which is not limited here.
[0148] In some embodiments, the mixed coating fluid includes a polar solvent.
[0149] In some embodiments, the polar solvent includes at least one of water, anhydrous ethanol, methanol, and isopropanol.
[0150] In some embodiments, the mass ratio of the secondary particles to the polymer is 10:(0.1-5), specifically 10:0.1, 10:1, 10:2, 10:3, 10:4 or 10:5, which is not limited here.
[0151] In some embodiments, the drying temperature of spray drying is 60°C to 200°C, specifically 60°C, 80°C, 100°C, 120°C, 150°C, 180°C or 200°C.
[0152] In some embodiments, the polymer includes at least one of a diblock copolymer, a triblock copolymer, and a multiblock copolymer.
[0153] In some embodiments, the polymer includes at least one of polyacrylic acid, polyacrylonitrile, polyimide, polyurethane, polydopamine, xanthan gum, polypyrrole, polythiophene, polyphenylene vinylene, polyaniline, polyacetylene, and tannic acid.
[0154] In some embodiments, the step of surface coating the secondary particles with a coating material includes: introducing a second gas-phase carbon source into the secondary particles, heating the second gas-phase carbon source until a thermal cracking reaction occurs, so that the surface of the secondary particles is deposited to form a coating material, and the coating material includes at least one of an amorphous carbon material and a graphitized carbon material.
[0155] In some embodiments, the second gas-phase carbon source includes at least one of acetylene, methane, toluene, cyclohexane, ethanol, ethylene, and propylene.
[0156] In some embodiments, the heating rate of the thermal cracking reaction is 1°C / min to 20°C / min, specifically 1°C / min, 3°C / min, 5°C / min, 8°C / min, 10°C / min, 15°C / min or 20°C / min, which is not limited here.
[0157] In some embodiments, the temperature of the thermal cracking reaction is 600°C to 1000°C, specifically, the reaction temperature can be 600°C, 650°C, 700°C, 750°C, 800°C, 890°C, 900°C, 960°C or 1000°C. The inventors have found through multiple experiments that controlling the reaction temperature within 600°C to 1000°C can improve the reaction efficiency, so that a uniform carbon layer is formed on the surface of the secondary particles, and the carbon layer can be amorphous carbon. Preferably, the reaction temperature is 700°C to 900°C.
[0158] In some embodiments, the insulation time of the thermal cracking reaction is 1 h to 48 h; specifically, it can be 1 h, 4 h, 8 h, 12 h, 16 h, 24 h, 28 h, 32 h, 38 h or 48 h, which is not limited here.
[0159] In some embodiments, the concentration of the gaseous carbon source is 0.1 L / min to 10 L / min; specifically, it can be 0.1 L / min, 0.4 L / min, 0.6 L / min, 0.8 L / min, 1.0 L / min, 2 L / min, 5 L / min, 6 L / min, 8 L / min, 9 L / min or 10 L / min, etc., which is not limited here.
[0160] In some embodiments, the thermal cracking reaction is carried out under a protective atmosphere.
[0161] In some embodiments, the protective atmosphere includes at least one of helium, neon, argon, krypton, and xenon.
[0162] The embodiment of the present invention further provides a battery, using the negative electrode material provided by the above embodiment of the present invention or the negative electrode material prepared by the preparation method of the negative electrode material provided by the above embodiment of the present invention. The battery provided by the embodiment of the present invention has the advantages of high capacity, high initial efficiency, long cycle life, excellent rate performance and low expansion. The battery can be a lithium ion battery, a sodium ion battery, a solid electrolyte battery, etc., which is not limited here.
[0163] The following is a further description of the embodiments of the present invention in multiple embodiments. The embodiments of the present invention are not limited to the following specific embodiments. The embodiments can be appropriately modified within the scope of the unchanged main rights.
[0164] Example 1
[0165] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.06 Pa, and then heated to 1250°C at a heating rate of 3°C / min. The pressure was maintained at 5 Pa and kept warm for 4 hours to obtain an intermediate.
[0166] (2) The intermediate is placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 950°C at a heating rate of 3°C / min, kept at this temperature for 5 hours, and then cooled to obtain a precursor.
[0167] (3) Dissolve 100 g of the precursor in the prepared etching solution, and perform etching reaction for 2 h. Keep the reaction temperature below 30° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 12:3:1:4. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0168] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace, and heated to 950 ° C at a heating rate of 3 ° C / min under the protection of argon atmosphere, and then 0.5 L / min of acetylene gas was introduced so that the volume ratio of argon to acetylene in the rotary atmosphere furnace was 9:1. After keeping warm for 4 hours, the silicon-carbon composite was obtained by cooling.
[0169] (5) 10 g of the silicon-carbon composite was dissolved in 100 g of anhydrous ethanol, 1 g of polyacrylic acid was added, and mechanical stirring was performed for 30 minutes. The surface of the silicon-carbon composite was coated with the polymer by spray drying at a temperature of 100° C., thereby obtaining a negative electrode material.
[0170] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0171] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0172] Figure 3 is the XRD diagram of the negative electrode material in this embodiment, from Figure 3 It can be seen from the XRD spectrum that the three strong peaks at 28.4°, 47.3° and 56.1° correspond to the three strong peaks of silicon (JCPDS No.27-1402), and there is basically no impurity phase. According to the Scherrer formula, the silicon grain size is calculated to be 3.5nm.
[0173] Figure 4a and Figure 4b They are respectively a scanning electron microscope image and an internal cross-sectional view of the negative electrode material prepared in Example 1. Figure 4a and Figure 4b As shown, the surface of the negative electrode material has a dense carbon coating layer.
[0174] Figure 5a is a transmission electron microscope image of the negative electrode material in this embodiment, Figure 5b is a partial enlarged transmission electron microscope image of the negative electrode material in this embodiment, such as Figure 5a and Figure 5b As shown, the primary particles inside the negative electrode material are evenly distributed in the carbon matrix.
[0175] Figure 6 is the cycle performance curve of the negative electrode material in this embodiment, such as Figure 6 As shown, the negative electrode material has excellent cycle performance, with a capacity retention rate of 93.8% after 50 cycles at a current of 0.25C.
[0176] Example 2
[0177] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.03 Pa, and then heated to 1250°C at a heating rate of 1°C / min. The pressure was maintained at 3Pa and kept warm for 6 hours to obtain an intermediate.
[0178] (2) The intermediate is placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 750°C at a heating rate of 1°C / min, kept at this temperature for 12 hours, and then cooled to obtain a precursor.
[0179] (3) Dissolve 100 g of the precursor in the prepared etching solution, and perform etching reaction for 2 h. Keep the reaction temperature below 30° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 12:3:1:4. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0180] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace and heated to 750 °C at a heating rate of 3 °C / min under the protection of an argon atmosphere. Then, 4.5 L / min of propane gas was introduced so that the volume ratio of argon to propane in the rotary atmosphere furnace was 9:1. After keeping the temperature for 4 h, the furnace was cooled to obtain a silicon-carbon composite.
[0181] (5) Take 10 g of the silicon-carbon composite and place it in a rotary atmosphere furnace. Under the protection of an argon atmosphere, heat it to 600°C at a heating rate of 1°C / min, then introduce 0.2 L / min of propane gas so that the volume ratio of argon to propane in the rotary atmosphere furnace is 9:1. After keeping the temperature for 6 hours, turn off the propane gas and cool it to obtain the negative electrode material.
[0182] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0183] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0184] Embodiment 3:
[0185] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.01 Pa, and then heated to 1150°C at a heating rate of 1°C / min. The pressure was maintained at 2Pa and kept warm for 8 hours to obtain an intermediate.
[0186] (2) The intermediate is placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 650°C at a heating rate of 1°C / min, kept at this temperature for 12 hours, and then cooled to obtain a precursor.
[0187] (3) Dissolve 100 g of the precursor in 100 g of the prepared etching solution, and perform etching reaction for 2 h. Keep the reaction temperature below 20° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 6:3:1:3. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0188] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace, and heated to 650 ° C at a heating rate of 3 ° C / min under the protection of argon atmosphere, and then 5.5 L / min of propane gas was introduced so that the volume ratio of argon to propane in the rotary atmosphere furnace was 9:1. After keeping warm for 8 hours, the silicon-carbon composite was obtained by cooling.
[0189] (5) 10 g of the silicon-carbon composite was dissolved in 100 g of anhydrous ethanol, 1 g of polyacrylic acid was added, and mechanical stirring was performed for 30 minutes. The surface of the silicon-carbon composite was coated with the polymer by spray drying at a temperature of 110° C., thereby obtaining a negative electrode material.
[0190] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0191] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0192] Example 4
[0193] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.075 Pa, and then heated to 1650°C at a heating rate of 10°C / min. The pressure was maintained at 9 Pa and kept warm for 8 hours to obtain an intermediate.
[0194] (2) The intermediate is placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 1050°C at a heating rate of 30°C / min, kept at this temperature for 12 hours, and then cooled to obtain a precursor.
[0195] (3) Dissolve 100 g of the precursor in 100 g of the prepared etching solution, and perform etching reaction for 2 h. Keep the reaction temperature below 20° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 6:3:1:3. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0196] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace, and heated to 950 °C at a heating rate of 5 °C / min under the protection of an argon atmosphere. Then, 2 L / min of propane gas was introduced so that the volume ratio of argon to propane in the rotary atmosphere furnace was 9:1. After keeping the temperature for 8 h, the furnace was cooled to obtain a silicon-carbon composite.
[0197] (5) 100 g of the silicon-carbon composite was placed in a rotary atmosphere furnace. Under the protection of an argon atmosphere, the temperature was increased to 950 °C at a rate of 10 °C / min, and 4 L / min of acetylene gas was introduced so that the volume ratio of argon to acetylene in the rotary atmosphere furnace was 9:1. After keeping the temperature for 6 h, the acetylene gas was turned off and the anode material was obtained by cooling.
[0198] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0199] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0200] Example 5
[0201] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.075 Pa, and then heated to 1650°C at a heating rate of 10°C / min. The pressure was maintained at 9 Pa and kept warm for 8 hours to obtain an intermediate.
[0202] (2) The intermediate is placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 1000°C at a heating rate of 30°C / min, kept at this temperature for 12 hours, and then cooled to obtain a precursor.
[0203] (3) Dissolve 100 g of the precursor in 100 g of the prepared etching solution, and perform etching reaction for 2 h. Keep the reaction temperature below 20° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 6:3:1:3. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0204] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace. Under the protection of an argon atmosphere, the furnace was heated to 1000° C. at a heating rate of 5° C. / min. Then, 2 L / min of propane gas was introduced so that the volume ratio of argon to propane in the rotary atmosphere furnace was 9:1. After keeping the temperature for 8 h, the furnace was cooled to obtain a silicon-carbon composite.
[0205] (5) 100 g of silicon-carbon composite was placed in a rotary atmosphere furnace. Under the protection of argon atmosphere, the temperature was increased to 1000 °C at a rate of 10 °C / min. Then, 4 L / min of acetylene gas was introduced so that the volume ratio of argon to acetylene in the rotary atmosphere furnace was 9:1. After keeping the temperature for 6 h, the acetylene gas was turned off and the anode material was obtained by cooling.
[0206] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0207] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0208] Example 6
[0209] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.075 Pa, and then heated to 1550°C at a heating rate of 10°C / min. The pressure was maintained at 9 Pa and kept warm for 7 hours to obtain an intermediate.
[0210] (2) The intermediate is placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 600°C at a heating rate of 1°C / min, kept at this temperature for 24 hours, and then cooled to obtain a precursor.
[0211] (3) Dissolve 100 g of the precursor in 100 g of the prepared etching solution, and perform etching reaction for 2 h. Keep the reaction temperature below 20° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 6:3:1:3. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0212] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace. Under the protection of an argon atmosphere, the furnace was heated to 600 °C at a heating rate of 5 °C / min, and then 3 L / min of propane gas was introduced so that the volume ratio of argon to propane in the rotary atmosphere furnace was 9:1. After keeping the temperature for 8 h, the furnace was cooled to obtain a silicon-carbon composite.
[0213] (5) 100 g of silicon-carbon composite was placed in a rotary atmosphere furnace. Under the protection of argon atmosphere, the temperature was increased to 600 °C at a rate of 1 °C / min. Then, 4 L / min of acetylene gas was introduced so that the volume ratio of argon to acetylene in the rotary atmosphere furnace was 9:1. After keeping the temperature for 6 h, the acetylene gas was turned off and cooled to obtain the negative electrode material.
[0214] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0215] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0216] Example 7
[0217] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:1 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.06 Pa, and then heated to 1250°C at a heating rate of 10°C / min. The pressure was maintained at 5 Pa and kept warm for 6 hours to obtain an intermediate.
[0218] (2) The intermediate was placed in an atmosphere furnace, and under the protection of an argon atmosphere, heated to 700°C at a heating rate of 1°C / min, kept at that temperature for 18 hours, and then cooled to obtain a precursor.
[0219] (3) Dissolve 100 g of the precursor in 100 g of the prepared etching solution, and perform etching reaction for 4 h. Keep the reaction temperature below 20° C. during the entire etching process. The etching solution uses a mixed solution of hydrofluoric acid: water: ethanol: ammonium fluoride with a mass ratio of 6:3:1:3. After the reaction is completed, centrifuge and dry to obtain silicon particles with holes.
[0220] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace, and heated to 700 °C at a heating rate of 5 °C / min under the protection of an argon atmosphere. Then, 2 L / min of acetylene gas was introduced so that the volume ratio of argon to acetylene in the rotary atmosphere furnace was 9:1. After keeping the temperature for 12 h, the furnace was cooled to obtain a silicon-carbon composite.
[0221] (5) Take 100 g of silicon-carbon composite and place it in a rotary atmosphere furnace. Under the protection of argon atmosphere, heat it to 700 °C at a heating rate of 1 °C / min, then introduce 4 L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After keeping warm for 3 hours, turn off the acetylene gas and cool it to obtain the negative electrode material.
[0222] The negative electrode material prepared in this embodiment includes secondary particles and a coating material located on at least part of the surface of the secondary particles, wherein the coating material is a polymer; the secondary particles include mutually dispersed carbon materials and primary particles, wherein the primary particles include a plurality of silicon grains.
[0223] The remaining parameters of the negative electrode material in this embodiment are detailed in Table 1.
[0224] Example 8
[0225] The difference from Example 1 is:
[0226] (1) Silicon powder and silicon micropowder (SiO2) were mixed evenly in a molar ratio of 1:0.9 and placed in a vacuum sintering furnace. The vacuum high-temperature sintering furnace was evacuated to 0.06 Pa, and then heated to 1250°C at a heating rate of 3°C / min. The pressure was maintained at 5 Pa and kept warm for 4 hours to obtain an intermediate.
[0227] Example 9
[0228] The difference from Example 1 is:
[0229] (4) 500 g of silicon particles were placed in a rotary atmosphere furnace. Under the protection of an argon atmosphere, the furnace was heated to 950 °C at a heating rate of 3 °C / min, and 0.5 L / min of acetylene gas was introduced so that the volume ratio of argon to acetylene in the rotary atmosphere furnace was 9:1. After keeping the temperature for 8 h, the furnace was cooled to obtain the negative electrode material.
[0230] Comparative Example 1
[0231] (1) 100 g of porous carbon material with an average size of 8 um was placed in an atmosphere furnace filled with a protective atmosphere, and the temperature was raised to 700 ° C at a heating rate of 3 ° C / min, and 0.5 L / min of silane gas was introduced. After keeping the temperature for 3 hours, the silicon-carbon composite was taken out after cooling to room temperature; wherein the average pore size of the porous carbon material is between 2-100 nm.
[0232] (2) After grinding and grading the silicon-carbon composite, 100 g of the silicon-carbon composite was dissolved in 100 g of anhydrous ethanol, 1 g of polyacrylic acid was added, and mechanical stirring was performed for 30 minutes. The drying temperature was controlled at 100° C. by spray drying so that the surface of the silicon-carbon composite was coated with the polymer to prepare a negative electrode material.
[0233] Performance Testing
[0234] 1) Average particle size of negative electrode material:
[0235] The average particle size test method of the secondary particles refers to GB / T 19077-2016, and is measured using a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK, and the median particle size is used to represent the average particle size.
[0236] 2) Testing method for specific surface area of negative electrode material:
[0237] The equipment used is the TriStar3000&3020 fully automatic specific surface and pore size analyzer from Micromeritics Inc. of the United States, which complies with the national standard GB / T 19587-2017. Under constant temperature and low temperature, the adsorption amount of gas on the solid surface at different relative pressures is measured, and then the monolayer adsorption amount of the sample is obtained based on the Brownauer-Etter-Taylor adsorption theory and its formula (BET formula), thereby calculating the specific surface area of the material.
[0238] 3) Testing method of tap density:
[0239] The tap density of powders was tested using the DAT-6-220 powder tap density instrument from Kantar Corporation of the United States. According to the national standard GB / T 5162-2006 / ISO 3953:1993, a certain amount of sample was weighed and the tap density was tested at 300 times / min and 3000 vibrations.
[0240] 4) Test methods for oxygen content and carbon content:
[0241] The oxygen content was measured by a Nicolet Is10 Fourier transform infrared spectrometer from Thermo Fisher, USA, and the carbon layer content was tested by thermogravimetric analysis.
[0242] 5) SEM test:
[0243] The scanning electron microscopy characterization was carried out on a S4800 field emission electron microscope of Hitachi Company, Japan, with an operating voltage of 200 kV, to observe the structure of the negative electrode material and to scale the thickness of the coating layer.
[0244] 6) Test method for average size of primary particles:
[0245] The average particle size was measured using an E3500 ion mill and an S4800 field emission electron microscope from Hitachi, Japan.
[0246] 7) Testing method for average particle size of silicon grains:
[0247] The XRD spectrum of the sample was measured by TD-3600 X-ray diffractometer of Tongda Company in Dandong, China. The half-maximum width of the diffraction peak of the sample and the corresponding Bragg angle were obtained by jade software. The average grain size of the silicon grains was calculated by Scherrer formula D=Kγ / B cosθ, and the obtained average grain size was used to represent the average grain diameter.
[0248] 8) Testing method for coating thickness:
[0249] The material was sectioned using an E3500 ion mill and an S4800 field emission electron microscope from Hitachi, Japan, and the thickness of the particle modification layer and the protective layer were measured in SEM.
[0250] 9) Testing method for particle size of negative electrode material:
[0251] D50 was measured using a laser particle size analyzer, and it had a symmetrical distribution similar to a normal distribution. In its volume reference distribution, the cumulative 50% diameter is D50, and by analogy, the cumulative 90% diameter is D90, and the cumulative 10% diameter is D10.
[0252] After the above tests, the negative electrode materials prepared in Examples 1 to 9 and Comparative Example 1 have sample numbers corresponding to S1 to S9 and R1; the performance parameters of the negative electrode materials are shown in Table 1:
[0253] Table 1. Performance parameters of negative electrode materials
[0254]
[0255] 10) Electrochemical test:
[0256] The negative electrode material was mixed with sodium carboxymethyl cellulose, styrene-butadiene rubber, conductive graphite (KS-6) and carbon black (SP) in a ratio of 92:2:2:2:2 to prepare a slurry, uniformly coated on a copper foil and dried to make a negative electrode sheet, which was assembled into a button cell in an argon atmosphere glove box. The separator used was a polypropylene microporous membrane, the electrolyte used was 1 mol / L lithium hexafluorophosphate (the solvent was a mixture of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate), and the counter electrode used was a metal lithium sheet.
[0257] The above 10 groups of batteries were tested for discharge specific capacity on a Blue Power CT2001A battery testing system. The ratio of the amount of electricity discharged in one hour to the battery capacity is the discharge specific capacity.
[0258] The above 10 groups of batteries were subjected to the first coulombic efficiency test on the Blue Power CT2001A battery testing system, with the charge and discharge current being 0.05C, and the first coulombic efficiency was measured.
[0259] The above 10 groups of batteries were tested for 100 cycles on a Blue Power CT2001A battery testing system with a charge and discharge current of 0.2C. After 100 cycles, the battery capacity and capacity retention rate after the cycle were calculated.
[0260] Among them, the capacity retention rate after 100 cycles at 0.2C = 100th cycle discharge capacity / first cycle discharge capacity*100%. The results are shown in Table 2.
[0261] Table 2 Parameter performance comparison of each battery
[0262]
[0263] As shown in Table 2, the negative electrode materials prepared in Examples 1 to 9 can reduce the grain boundary surface energy of the primary particles by controlling the crystallization instability of the negative electrode materials to F, 0.01≤F≤500, can weaken the stress concentration phenomenon generated by the primary particles during the lithium insertion and deinsertion process, improve the electrochemical sintering phenomenon of the negative electrode materials after lithium insertion, improve the structural stability of the primary particles during the lithiation process, reduce the expansion rate of the negative electrode materials, and be conducive to forming a stable solid electrolyte membrane, thereby improving the electrochemical performance of the negative electrode materials; in addition, in the secondary particles of the negative electrode materials, the carbon material and the primary particles are dispersed with each other, which can effectively improve the conductivity of the primary particles and can also effectively alleviate the volume expansion of the primary particles; part of the carbon material is located on the surface of the secondary particles, which can further alleviate the volume expansion of the negative electrode material, and can also effectively reduce the side reaction of the primary particles with the electrolyte, while enhancing the structural stability of the negative electrode material, so that the negative electrode material has low expansion, high cycle stability, high rate performance and high first coulomb efficiency.
[0264] During the preparation process of the negative electrode material of Comparative Example 1, the crystallization instability F of the negative electrode material is too large, which means that the size of the silicon grains is too small, and electrochemical sintering is prone to occur on the surface of the primary particles. After sintering, the silicon grains grow, and lithium insertion causes the local stress of the primary particles to increase. The instability of the entire structure is enhanced, resulting in reduced cycle performance and capacity of the negative electrode material, and deterioration of the electrochemical performance of the negative electrode material.
Claims
1. A negative electrode material, characterized in that: comprising secondary particles, the secondary particles comprising mutually dispersed carbon materials and primary particles, the primary particles comprising at least one silicon grain; The average particle size of silicon crystals of the negative electrode material measured at 25°C is M0 nm, 0.1≤M0≤20; the average particle size of silicon crystals of the negative electrode material measured at 25°C after being heated to 1000°C at a heating rate of 5°C / min under nitrogen protection and then kept warm for 1h and naturally cooled to 25°C is M1 nm, 5≤M1≤50; The crystal instability of the negative electrode material is F, where F=(M1-M0) / M0, M1>M0, and 0.01≤F≤500.
2. The negative electrode material according to claim 1, characterized in that Contains at least one of the following characteristics: (1) The average particle size of the primary particles is 1 nm to 100 nm; (2) The pore volume of the negative electrode material is 0.01 cm 3 / g~0.2cm 3 / g; (3) The mass content of oxygen in the negative electrode material is less than 15%; (4) The mass content of silicon in the negative electrode material is 40% to 80%; (5) The carbon material includes at least one of amorphous carbon and graphitized carbon.
3. The negative electrode material according to claim 1, characterized in that It also includes a coating material located on at least part of the surface of the secondary particles, and the negative electrode material meets at least one of the following characteristics: (1) The coating material includes at least one of an amorphous carbon material, a graphitized carbon material, and a polymer; (2) The coating material comprises a polymer, and the polymer comprises at least one of polyacrylic acid, polyacrylonitrile, polyimide, polyurethane, polydopamine, xanthan gum, polypyrrole, polythiophene, polyphenylene vinylene, polyaniline, polyacetylene, and tannic acid; (3) The coating material comprises a polymer, and the thickness of the coating layer formed by the coating material is 50 nm to 300 nm; (4) The coating material comprises a graphitized carbon material, and the thickness of the coating layer formed by the coating material is 5 nm to 100 nm; (5) The coating material includes an amorphous carbon material, and the coating layer formed by the coating material has a thickness of 10 nm to 500 nm.
4. The negative electrode material according to any one of claims 1 to 3, characterized in that The negative electrode material meets at least one of the following characteristics: (1) The mass content of carbon in the negative electrode material is 5% to 80%; (2) The tap density of the negative electrode material is 0.3 g / cm 3 ~1.3g / cm 3 ; (3) The powder compaction density of the negative electrode material is 1.2 g / cm 3 ~1.8g / cm 3 ; (4) The median particle size of the negative electrode material is 0.5 μm to 26 μm; (5) The specific surface area of the negative electrode material is 0.8 m 2 / g~40m 2 / g.
5. A method for preparing the negative electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The mixture containing silicon element powder and silicon micropowder is subjected to a sintering treatment to obtain an intermediate; The intermediate is subjected to secondary sintering treatment, so that the intermediate undergoes a disproportionation reaction to obtain a precursor; Placing the precursor in an etching solution for etching to obtain silicon particles with holes; The silicon particles having pores are subjected to vapor phase carbon deposition using a first vapor phase carbon source to obtain secondary particles, and the negative electrode material includes the secondary particles.
6. The preparation method according to claim 5, characterized in that: The preparation method meets at least one of the following characteristics: (1) The mass content of oxygen in the silicon powder is ≤5%; (2) The molar ratio of the silicon element powder to the silicon micropowder is 1:(0.9-1.1); (3) The temperature of the primary sintering treatment is 1150° C. to 1650° C.; (4) The time of the primary sintering treatment is 3 h to 12 h; (5) The heating rate of the primary sintering treatment is 1°C / min to 20°C / min; (6) The pressure of the primary sintering treatment is ≤10Pa; (7) The temperature of the secondary sintering treatment is 200° C. to 1050° C.; (8) The secondary sintering treatment time is 1h to 48h; (9) The heating rate of the secondary sintering treatment is 1°C / min to 30°C / min.
7. The preparation method according to claim 5, characterized in that: The preparation method meets at least one of the following characteristics: (1) The mass ratio of the precursor to the etching solution is 1:(5-20); (2) The etching solution includes hydrofluoric acid, water, ethanol and ammonium fluoride; (3) The etching solution comprises hydrofluoric acid, water, ethanol and ammonium fluoride, wherein the mass ratio of the hydrofluoric acid, the water, the ethanol and the ammonium fluoride is (6-24):3:1:(3-6); (4) The etching solution comprises hydrofluoric acid, water, ethanol and ammonium fluoride, wherein the mass concentration of the hydrofluoric acid is 40%; (5) The etching reaction time is 0.5h to 10h; (6) The temperature of the etching reaction is ≤40°C; (7) The method further comprises washing and drying the etching reaction product; (8) The mass content of oxygen in the silicon particles having pores is less than 5%; (9) The mass content of water in the silicon particles having pores is less than 1%.
8. The method for preparing the negative electrode material according to claim 5, characterized in that: The preparation method meets at least one of the following characteristics: (1) The heating rate of the vapor phase carbon deposition is 1°C / min to 30°C / min; (2) The reaction temperature of the vapor phase carbon deposition is 200°C to 1050°C; (3) The holding time of the vapor phase carbon deposition is 1 h to 48 h; (4) the first gaseous carbon source comprises at least one of acetylene, methane, ethylene, propane, toluene, cyclohexane, ethanol, ethylene, propylene, pyrrole and acetonitrile; (5) The flow rate of the first gas-phase carbon source is 0.1 L / min to 10 L / min.
9. The method for preparing the negative electrode material according to claim 5, characterized in that: The method further comprises: performing surface coating treatment on the secondary particles using a coating material, which satisfies at least one of the following characteristics: (1) The coating material includes at least one of an amorphous carbon material, a graphitized carbon material, and a polymer; (2) the step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; (3) The step of coating the surface of the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the solid content of the secondary particles in the mixed coating liquid is 5% to 50%; (4) The step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the mixed coating liquid comprises a polar solvent; (5) The step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the polar solvent comprises at least one of water, anhydrous ethanol, methanol and isopropanol; (6) The step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the mass ratio of the secondary particles to the polymer is 10:(0.1-5); (7) The step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the drying temperature of the spray drying is 60° C. to 200° C.; (8) The step of coating the secondary particles with a coating material comprises: spray drying a mixed coating liquid containing the secondary particles and a polymer; wherein the polymer comprises at least one of polyacrylic acid, polyacrylonitrile, polyimide, polyurethane, polydopamine, xanthan gum, polypyrrole, polythiophene, polyphenylene vinylene, polyaniline, polyacetylene and tannic acid; (9) The step of coating the secondary particles with a coating material comprises: introducing a second gas-phase carbon source into the secondary particles, heating the second gas-phase carbon source until the second gas-phase carbon source undergoes a thermal cracking reaction, so that the second gas-phase carbon source is deposited on the surface of the secondary particles to form a coating material, wherein the coating material comprises at least one of an amorphous carbon material and a graphitized carbon material; (10) The step of coating the secondary particles with a coating material comprises: introducing a second gas-phase carbon source into the secondary particles, heating the second gas-phase carbon source until the second gas-phase carbon source undergoes a thermal cracking reaction, so that the second gas-phase carbon source is deposited on the surface of the secondary particles to form a coating material, wherein the gas-phase carbon source comprises at least one of acetylene, methane, toluene, cyclohexane, ethanol, ethylene and propylene; (11) The step of coating the secondary particles with a coating material comprises: introducing a second gaseous carbon source into the secondary particles, heating the second gaseous carbon source until the second gaseous carbon source undergoes a thermal cracking reaction, so that the second gaseous carbon source is deposited on the surface of the secondary particles to form a coating material, wherein the concentration of the gaseous carbon source is 0.1 L / min to 10 L / min; (12) The step of using a coating material to coat the surface of the secondary particles comprises: introducing a second gas-phase carbon source into the secondary particles, heating the second gas-phase carbon source until a thermal cracking reaction occurs, so that the coating material is deposited on the surface of the secondary particles, the thermal cracking reaction temperature is 600°C to 1000°C, and the insulation time is 1h to 48h.
10. A battery, characterized in that: The invention comprises the negative electrode material according to any one of claims 1 to 4 or the negative electrode material prepared according to the method for preparing the negative electrode material according to any one of claims 5 to 9.
Citation Information
Patent Citations
Porous silicon composite cluster structure, method of preparing the same, carbon composite using the same, and electrode, lithium battery, and device each including the same
CN108075117A
Silicon-based negative electrode material for lithium ion battery and preparation method of silicon-based negative electrode material
CN109524626A
Soft carbon-hard carbon-silicon composite negative electrode material and preparation method thereof
CN115360334A
Negative electrode material, preparation method thereof and battery
CN117038945A
Silicon carbone compound negative polar material of lithium ion battery and its preparation method
CN1913200A