A flower-shaped nickel-cobalt-aluminum layered oxide catalyst and its preparation method and application

By preparing the floral spherical nickel-cobalt-aluminum layered oxide catalyst combined with persulfate, the problem of unstable structure of layered nickel-cobalt-aluminum oxide is solved, and efficient degradation of neonicotinoid insecticides in water is achieved, avoiding the Secondary pollution, suitable for large-scale production.

CN117920221BActive Publication Date: 2024-12-03NORTHEAST AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410028413.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-08
Publication Date
2024-12-03
Estimated Expiration
2044-01-08

AI Technical Summary

Technical Problem

In the prior art, the layered nickel-cobalt aluminum oxide structure is unstable, resulting in low catalytic activity and high reaction barrier, making it difficult to effectively degrade neonicotinoid insecticides in water. The commonly used chemical oxidation methods have high energy consumption and oxidant utilization. Low rate and secondary pollution problems.

Method used

The preparation method of a floral spherical nickel-cobalt-aluminum layered oxide catalyst is used to prepare nickel-cobalt-aluminum layered oxide through hydrothermal reaction and high-temperature calcination, and combined with persulfate to catalyze it to activate neonicotinoid insecticides in water. degradation.

Benefits of technology

Improve the structural and performance stability of the catalyst, increase the specific surface area, promote electron transfer, and achieve efficient degradation of neonicotinoid pesticides. It has a wide range of application, simple operation, avoids secondary pollution, and is suitable for scale. Production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117920221B_ABST
    Figure CN117920221B_ABST
Patent Text Reader

Abstract

The invention discloses a flower-ball-shaped nickel-cobalt-aluminum layered oxide catalyst and a preparation method and application thereof, and belongs to the technical field of sewage treatment. A solution containing a nickel salt, a cobalt salt, an aluminum salt, an alkaline substance and a template is stirred and subjected to a hydrothermal reaction, and the obtained solid nickel-cobalt-aluminum layered hydroxide is calcined to obtain a flower-ball-shaped nickel-cobalt-aluminum layered oxide catalyst. The nickel-cobalt-aluminum layered oxide prepared by the present invention has a stable structure and performance, has a flower-ball-shaped structure, can accelerate electron transfer, and when used for catalytic activation of persulfate to degrade neonicotinoid insecticides in water, improves the degradation efficiency of neonicotinoid insecticides in water. The degradation method has a wide pH application range, does not require additional energy, is simple to operate, and can effectively solve the problems of high pH requirements of the classical Fenton method, potential safety hazards in the transportation of hydrogen peroxide, and easy secondary pollution. Therefore, it has good application prospects in treating water bodies contaminated by neonicotinoid insecticides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sewage treatment, and in particular relates to a flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst and a preparation method and application thereof. Background Art

[0002] Neonicotinoids are a type of effective chlorinated neonicotinoid insecticide widely used in agriculture. Their accumulation in the environment not only reduces the reproductive capacity of pollinators, but also poses a chronic risk to human health. Most neonicotinoid insecticides cannot be completely decomposed in the soil. These neonicotinoid insecticides can easily enter water sources, including streams, rivers and groundwater. Since neonicotinoid insecticides have high water solubility, they are difficult to be degraded when discharged into water bodies, which will directly or indirectly affect human health and the ecological environment.

[0003] At present, treatment methods such as adsorption, flocculation, and biological treatment have been maturely applied to the treatment of refractory wastewater, but these methods often have unsatisfactory removal effects. For some commonly used chemical oxidation methods, such as chemical oxidation methods using chlorine and potassium permanganate as oxidants, although they can effectively remove refractory pollutants in wastewater, they have disadvantages such as high energy consumption, low oxidant utilization rate, large secondary pollution, and low removal efficiency in practical applications. Therefore, advanced oxidation technologies with advantages such as high utilization rate and low secondary pollution have received widespread attention in recent years and have gradually transitioned to practical applications. Persulfate advanced oxidation technology has received widespread attention in the field of water treatment because its sulfate radical has a higher redox potential than hydroxyl radicals.

[0004] Layered metal hydroxides (LDHs) are two-dimensional anionic clay materials whose basic structural unit is an octahedron. The layered metal oxides (LDOs) obtained after high-temperature calcination have a large specific surface area and more catalytic active sites, which can efficiently activate persulfate. Among the many catalysts for degrading neonicotinoid pesticides in water, nickel-based and cobalt-based catalysts have attracted much attention due to their strong electron transfer ability and low cost in bimetallic redox cycles. However, the structure of nickel-based and cobalt-based oxides is unstable, so further improving their catalytic activity, reducing the reaction barrier, and increasing the intrinsic conductivity and active site density is a difficult problem in this field. Summary of the invention

[0005] In order to solve the above problems in the prior art, the present invention provides a flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst and a preparation method and application thereof, so as to solve the problem of unstable structure of layered nickel-cobalt-aluminum oxide in the prior art.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a method for preparing a flower-spherical nickel-cobalt-aluminum layered oxide catalyst, comprising the following steps: stirring a solution containing a nickel salt, a cobalt salt, an aluminum salt, an alkaline substance and a template agent and performing a hydrothermal reaction, and calcining the obtained solid nickel-cobalt-aluminum layered hydroxide to obtain the flower-spherical nickel-cobalt-aluminum layered oxide catalyst.

[0008] As a preferred embodiment of the present invention, the nickel salt includes at least one of NiCl2, Ni(NO3)2 and Ni(CH3COO)2, the cobalt salt includes at least one of CoCl2, Co(NO3)2 and Co(CH3COO)2, the aluminum salt includes at least one of AlCl3, Al(NO3)3 and Al2(SO4)3, the alkaline substance includes urea and ammonia water, and the template includes hexadecyltrimethylammonium bromide.

[0009] Urea and ammonia are alkaline substances, which provide an alkaline environment and adjust the solution pH to 9-10, which is weakly alkaline. Other strong alkaline substances such as NaOH cannot make the resulting catalyst form a flower ball morphology. This is because when urea and ammonia provide an alkaline environment, the reaction is easy to control. The alkalinity of NaOH is too strong, which may cause the precipitate to dissolve again during the precipitation process, resulting in losses, and introduce new Na impurities.

[0010] Hexadecyltrimethylammonium bromide acts as a template and surfactant. Hexadecyltrimethylammonium bromide is used as a template. By maintaining the growth direction and size distribution of NiCoAl-LDO, the corresponding nickel salt, cobalt salt and aluminum source are mixed with it and placed in a high-pressure reactor for hydrothermal reaction to obtain a precursor. The precursor is calcined at high temperature to obtain NiCoAl-LDO with a flower ball morphology. The morphological effect is not good when other templates and surfactants are used, and the flower ball morphology of the obtained catalyst is not obvious.

[0011] As a preferred embodiment of the present invention, in the solution, the concentration of nickel salt is 0.025-0.25 mol / L, the concentration of cobalt salt is 0.025-0.25 mol / L, and the concentration of aluminum salt is 0.01-0.1 mol / L; in the solution, the molar ratio of nickel salt, cobalt salt and aluminum salt is (0.1-3):(0.1-3):1.

[0012] As a preferred embodiment of the present invention, in the solution, the concentration of the alkaline substance is 0.12-1.2 mol / L, and the concentration of the template agent is 0.01-0.1 mol / L.

[0013] As a preferred embodiment of the present invention, the hydrothermal temperature is 60-160°C, the hydrothermal reaction time is 6-16h; the calcination temperature is 300-600°C, the time is 0.5-2h, and the heating rate during heating to the calcination temperature is 2-15°C / min.

[0014] The present invention also provides a flower-spherical nickel-cobalt-aluminum layered oxide catalyst prepared according to the preparation method of the flower-spherical nickel-cobalt-aluminum layered oxide catalyst described above.

[0015] The present invention also provides an application of the above-mentioned flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst in degrading neonicotinoid pesticides in water.

[0016] As a preferred embodiment of the present invention, the application includes the following steps: adding the flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst and persulfate to water containing neonicotinoid insecticides, and performing a shock reaction to complete the degradation treatment of the neonicotinoid insecticides in the water.

[0017] As a preferred embodiment of the present invention, in the water containing neonicotinoid insecticides, the concentration of neonicotinoid insecticides is 1-20 mg / L, the concentration of the flower ball-shaped nickel cobalt aluminum layered oxide catalyst is 0.1-1.5 g / L, and the concentration of persulfate is 0.5-5 mM; and the reaction time is 0.5 h.

[0018] As a preferred embodiment of the present invention, the persulfate includes at least one of sodium persulfate, potassium persulfate, sodium peroxymonosulfate, potassium peroxymonosulfate and potassium hydrogen persulfate.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention prepares a flower ball-shaped NiCoAl layered oxide, which has a more stable structure and performance; the NiCoAl layered oxide is specifically a flower ball-shaped structure, which can provide a larger specific surface area, reduce the overflow of metal ions, and accelerate electron transfer. When used for catalytic activation of persulfate to degrade neonicotinoid insecticides in water, the degradation efficiency of neonicotinoid insecticides in water is improved. The degradation method has a wide pH application range, can efficiently degrade in the pH range of 4 to 10, does not require additional energy, and is simple to operate. The method can effectively solve the problems of high pH requirements of the classical Fenton method, potential safety hazards in the transportation of hydrogen peroxide, and easy secondary pollution. Therefore, it has good application prospects in treating water bodies contaminated by neonicotinoid insecticides.

[0021] (2) The NiCoAl layered oxide prepared by the present invention has been experimentally confirmed to be able to effectively resist the influence of the water matrix on the degradation of neonicotinoid insecticides when used in combination with persulfate, for example, it can overcome the common Cl - , SO4 2-In actual water bodies, it also has good degradation ability for neonicotinoid insecticides. At the same time, the process for preparing NiCoAl layered oxides of the present invention is simple, has no secondary pollution, and is suitable for large-scale production.

[0022] (3) The present invention not only provides a new type of catalyst for the efficient degradation of neonicotinoid pesticides in water, but also generates a flower-shaped NiCoAl layered oxide with stable structure and excellent performance, which provides a new idea for the design and controllable preparation of layered oxides. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 In the figure, (a) and (b) are Ni prepared in Example 1. 1.5 Co 1.5 Scanning electron microscope images of Al1-LDO at different magnifications;

[0025] Figure 2 Ni prepared in step (1) of Example 1 1.5 Co 1.5 Al1-LDH, Ni prepared in step (2) 1.5 Co 1.5 Al1-LDO and Ni after completing the degradation experiment of Example 1 1.5 Co 1.5 XRD pattern of Al1-LDO;

[0026] Figure 3 This is a comparison chart of the degradation effects of the catalysts prepared in Examples 1 to 4 and Comparative Examples 1 to 2 on imidacloprid in water;

[0027] Figure 4 This is a scanning electron microscope image of the Ni1Co2-LDO prepared in Comparative Example 3;

[0028] Figure 5 This is the effect of different catalyst dosages on the degradation of imidacloprid in water;

[0029] Figure 6 This is a graph showing the effect of different persulfate dosages on the degradation of imidacloprid in water;

[0030] Figure 7 The Ni prepared in Example 1 1.5 Co 1.5Stability and reusability test results of Al1-LDO;

[0031] Figure 8 The Ni prepared in Example 1 1.5 Co 1.5 The degradation effect of Al1-LDO on different types of neonicotinoid insecticides;

[0032] Fig. 9 This is the effect of different pH on the degradation of imidacloprid in water;

[0033] Fig.10 In the figure, (a) and (b) are Cl - , SO4 2- Graph showing the effect on the degradation of imidacloprid in water. DETAILED DESCRIPTION

[0034] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0035] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0036] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0039] The raw materials used in the following examples are all commercially available conventional raw materials, and are not particularly limited thereto, and will not be described again.

[0040] Example 1

[0041] The preparation steps of the flower-shaped NiCoAl layered oxide are as follows:

[0042] (1) 0.015 mol Ni(NO3)2·6H2O, 0.015 mol Co(NO3)2·6H2O, 0.01 mol Al(NO3)3·9H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were added to 100 mL of distilled water in sequence, stirred and mixed, and heated to 120°C for hydrothermal reaction for 10 h. Then, a solid product was separated, washed and dried to obtain NiCoAl layered hydroxide, denoted as Ni 1.5 Co 1.5 Al1-LDH;

[0043] (2) The NiCoAl layered hydroxide obtained in step (1) was heated to 500°C at a heating rate of 10°C / min in an air atmosphere and then kept at that temperature for 1 hour. After cooling, NiCoAl layered oxide was obtained, which was denoted as Ni 1.5 Co 1.5 Al1-LDO.

[0044] Figure 1 In the figure, (a) and (b) are Ni prepared in this example. 1.5 Co 1.5 Scanning electron microscope images of Al1-LDO at different magnifications, such as Figure 1 As shown, the prepared Ni 1.5 Co 1.5 The Al1-LDO has a flower ball-like morphology and a high specific surface area.

[0045] Figure 2 The Ni prepared in step (1) of this example is shown. 1.5 Co 1.5 Al1-LDH and Ni prepared in step (2) 1.5 Co 1.5 Al1-LDO (in Figure 2 China-Israel "Ni before degradation 1.5 Co 1.5 Al1-LDO”) XRD pattern, such as Figure 2 As shown, Ni 1.5 Co 1.5 The peaks of Al1-LDH and standard hydrotalcite almost completely correspond to each other, indicating that Ni1.5 Co 1.5 Al1-LDH, after calcination, Ni 1.5 Co 1.5 The layered structure of Al1-LDH gradually disintegrates with the removal of interlayer water, some ions and hydroxyl groups, and finally forms Ni 1.5 Co 1.5 Al1-LDO. X-ray images show typical crystalline-poor phase (111), (200), and (220) planes.

[0046] Degradation experiment:

[0047] Take 0.015g of Ni prepared in step (2) of Example 1 1.5 Co 1.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0071 g of sodium persulfate was added and the reaction was shaken for 30 min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 min. 1 mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in Figure 3 As shown, in this embodiment, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 84.3% within 30 minutes.

[0048] Completed the degradation experiment of Ni 1.5 Co 1.5 The XRD pattern of Al1-LDO is shown in Figure 2 As shown (in Figure 2 China-Israel "Ni after degradation 1.5 Co 1.5 Al1-LDO”), from Figure 2 It can be seen that the Ni after catalytic degradation reaction 1.5 Co 1.5 The XRD structure of Al1-LDO does not change significantly, which proves that Ni 1.5 Co 1.5 Al1-LDO material has good stability.

[0049] Example 2

[0050] The preparation steps of the flower-shaped NiCoAl layered oxide are as follows:

[0051] (1) 0.01 mol Ni(NO3)2·6H2O, 0.02 mol Co(NO3)2·6H2O, 0.01 mol Al(NO3)3·9H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 120° C. for hydrothermal reaction for 10 h, then a solid product was separated, the solid product was washed and dried, and cooled to obtain NiCoAl layered hydroxide;

[0052] (2) The NiCoAl layered hydroxide obtained in step (1) was heated to 500°C at a heating rate of 10°C / min in an air atmosphere and then kept at that temperature for 1 hour to obtain a flower ball-shaped NiCoAl layered oxide, which was recorded as Ni1Co2Al1-LDO.

[0053] Degradation experiment:

[0054] Take 0.015g of Ni1Co2Al1-LDO prepared in step (2), add it to 30mL of 10mg / L imidacloprid solution, then add 0.0071g of sodium persulfate, and shake the reaction for 30min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30min, 1mL of the suspension was sampled, and injected into a brown liquid chromatography injection bottle pre-added with 80μL of methanol through a 0.22μM organic filter membrane to terminate the reaction. The results are shown in Figure 3 As shown, in this embodiment, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 56.9% within 30 minutes.

[0055] Example 3

[0056] The preparation steps of flower-shaped NiCoAl layered oxide are as follows:

[0057] (1) 0.005 mol Ni(NO3)2·6H2O, 0.025 mol Co(NO3)2·6H2O, 0.01 mol Al(NO3)3·9H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 120° C. for hydrothermal reaction for 10 h, then a solid product was separated, and the solid product was washed and dried to obtain a NiCoAl layered hydroxide;

[0058] (2) The NiCoAl layered hydroxide obtained in step (1) was heated to 500°C at a heating rate of 10°C / min in an air atmosphere and then kept at that temperature for 1 hour. After cooling, NiCoAl layered oxide was obtained, which was denoted as Ni 0.5 Co 2.5 Al1-LDO.

[0059] Degradation experiment:

[0060] Take 0.015g of Ni prepared in step (2) 0.5 Co 2.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0071 g of sodium persulfate was added and the reaction was shaken for 30 min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 min. 1 mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in Figure 3 As shown, in this embodiment, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 50.3% within 30 minutes.

[0061] Example 4

[0062] The preparation steps of flower-shaped NiCoAl layered oxide are as follows:

[0063] (1) 0.025 mol Ni(NO3)2·6H2O, 0.005 mol Co(NO3)2·6H2O, 0.01 mol Al(NO3)3·9H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 120° C. for hydrothermal reaction for 10 h, then a solid product was separated, and the solid product was washed and dried to obtain a NiCoAl layered hydroxide;

[0064] (2) The NiCoAl layered hydroxide obtained in step (1) was heated to 500°C at a heating rate of 10°C / min in an air atmosphere and then kept at that temperature for 1 hour. After cooling, NiCoAl layered oxide was obtained, which was denoted as Ni 2.5 Co 0.5 Al1-LDO.

[0065] Degradation experiment:

[0066] Take 0.015g of Ni prepared in step (2) 2.5 Co 0.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0071 g of sodium persulfate was added and the reaction was shaken for 30 min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 min. 1 mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in Figure 3As shown, in this embodiment, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 46.9% within 30 minutes.

[0067] The catalysts prepared in Examples 2 to 4 were observed using a scanning electron microscope, and it was found that their morphology was also flower ball-like and had a high specific surface area.

[0068] After replacing 0.12 mol of urea in Examples 1 to 4 with 2.3 mL of 2.5 mol / L ammonia water, the obtained product morphology and degradation test results were substantially consistent with those of the corresponding Examples.

[0069] Comparative Example 1

[0070] The same as Example 1, except that 0.015 mol Co(NO3)2·6H2O in Example 1 is replaced by 0.015 mol Ni(NO3)2·6H2O, that is, the catalyst is prepared only with Ni(NO3)2·6H2O and Al(NO3)3·9H2O in this comparative example, and the specific steps are as follows:

[0071] (1) 0.03 mol Ni(NO3)2·6H2O, 0.01 mol Al(NO3)3·9H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 120° C. for hydrothermal reaction for 10 h, then a solid product was separated, and the solid product was washed and dried to obtain a NiAl layered hydroxide;

[0072] (2) The NiAl layered hydroxide obtained in step (1) is heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere and then kept at that temperature for 1 hour. After cooling, a NiAl layered oxide is obtained, which is recorded as Ni3Al1-LDO.

[0073] It was observed that the Ni3Al1-LDO prepared in this comparative example failed to form a flower ball shape.

[0074] Degradation experiment:

[0075] Take 0.015g of Ni3Al1-LDO prepared in step (2), add it to 30mL of 10mg / L imidacloprid solution, then add 0.0071g of sodium persulfate, and shake for 30min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30min, 1mL of the suspension was sampled, and injected into a brown liquid chromatography injection bottle pre-added with 80μL of methanol through a 0.22μM organic filter membrane to terminate the reaction. The results are as follows: Figure 3 As shown, in this comparative example, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 29.1% within 30 minutes.

[0076] Comparative Example 2

[0077] The same as Example 1, except that 0.015 mol Ni(NO3)2·6H2O in Example 1 is replaced by 0.015 mol Co(NO3)2·6H2O, that is, this comparative example only uses Co(NO3)2·6H2O and Al(NO3)3·9H2O to prepare the catalyst, and the specific steps are as follows:

[0078] (1) 0.03 mol Co(NO3)2·6H2O, 0.01 mol Al(NO3)3·9H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 120° C. for hydrothermal reaction for 10 h, then a solid product was separated, and the solid product was washed and dried to obtain a CoAl layered hydroxide;

[0079] (2) The CoAl layered hydroxide obtained in step (1) was heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere and then kept at that temperature for 1 h. After cooling, a CoAl layered oxide was obtained, which was recorded as Co3Al1-LDO.

[0080] It was observed that the Co3Al1-LDO prepared in this comparative example failed to form a flower ball shape.

[0081] Degradation experiment:

[0082] Take 0.015g of the Co3Al1-LDO prepared in step (2) and add it to 30mL of 10mg / L imidacloprid solution, then add 0.0071g of sodium persulfate and shake for 30min. During the catalytic reaction, samples were taken at 3, 5, 8, 15 and 30min, 1mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80μL of methanol through a 0.22μM organic filter membrane to terminate the reaction. The results are shown in Figure 3 As shown, in this comparative example, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 37.1% within 30 minutes.

[0083] Comparative Example 3

[0084] The same as Example 1, except that 0.015 mol Al(NO3)2·9H2O in Example 1 is replaced by 0.015 mol Co(NO3)2·6H2O, that is, the catalyst is prepared only with Ni(NO3)2·6H2O and Co(NO3)2·6H2O in this comparative example, and the specific steps are as follows:

[0085] (1) 0.015 mol Ni(NO3)2·6H2O, 0.03 mol Co(NO3)2·6H2O, 0.12 mol urea and 0.005 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 120° C. for hydrothermal reaction for 10 h, then a solid product was separated, and the solid product was washed and dried to obtain a NiCo layered hydroxide;

[0086] (2) The NiCo layered hydroxide obtained in step (1) is heated to 500°C at a heating rate of 10°C / min in an air atmosphere and then kept at that temperature for 1 hour. After cooling, a NiCo layered oxide is obtained, which is recorded as Ni1Co2-LDO.

[0087] The scanning electron microscope image of the Ni1Co2-LDO prepared in this comparative example is as follows Figure 4 As shown by Figure 4 It can be seen that the Ni1Co2-LDO prepared in this comparative example does not have a regular flower ball shape.

[0088] Degradation experiment:

[0089] Take 0.015g of Ni1Co2-LDO prepared in step (2), add it to 30mL of imidacloprid solution with a concentration of 10mg / L, then add 0.0071g of sodium persulfate, and oscillate for 30min. Samples are taken at 3, 5, 8, 15, and 30min during the catalytic reaction, 1mL is sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80μL of methanol through a 0.22μM organic filter membrane to terminate the reaction. In this comparative example, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid within 30min is 42.8%.

[0090] Embodiments 5 to 8

[0091] Degradation effect of different catalyst dosages on imidacloprid in water:

[0092] Take 0.003g, 0.009g, 0.03g and 0.045g of Ni prepared in step (2) of Example 1 respectively. 1.5 Co 1.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution (i.e., Ni 1.5 Co 1.5The concentrations of Al1-LDO were 0.1, 0.3, 1, and 1.5 g / L, respectively. Then, 0.0071 g of sodium persulfate was added and the reaction was shaken for 30 min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 min. 1 mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in Figure 5 As shown in the figure, 0.5 g / L is the degradation test result in Example 1. Figure 5 It can be seen that the degradation of imidacloprid conforms to the first-order kinetic equation. 1.5 Co 1.5 When the initial concentrations of Al1-LDO were 0.1, 0.3, 0.5, 1, and 1.5 g / L, the removal rates of imidacloprid within 30 min were 51.3%, 76.2%, 84.3%, 83.6%, and 84.3%, respectively.

[0093] Examples 9 to 12

[0094] Degradation effect of different persulfate dosages on imidacloprid in water:

[0095] Take 0.0015g of Ni prepared in step (2) of Example 1 1.5 Co 1.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0036 g, 0.014 g, 0.021 g and 0.036 g of sodium persulfate were added (i.e., the concentrations of sodium persulfate in the imidacloprid solution were 0.5, 2, 3 and 5 mM, respectively), and the reaction was oscillated for 30 min. During the catalytic reaction, samples were taken at 3, 5, 8, 15 and 30 min, 1 mL was sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in FIG. Figure 6 As shown in the figure, 1mM is the degradation experiment result in Example 1. Figure 6 It can be seen that the degradation of imidacloprid conforms to the first-order kinetic equation. When the initial concentrations of sodium persulfate in the imidacloprid solution are 0.5, 1, 2, 3, and 5 mM, respectively, the removal rates of imidacloprid within 30 min are 51.2%, 84.3%, 84.6%, 85.1%, and 87.8%, respectively. The initial concentration of sodium persulfate starts from 1 mM. As the concentration increases, the increase in the removal rate of imidacloprid within 30 min is not obvious. Therefore, considering the comprehensive cost and experimental plan, 1 mM is the best choice.

[0096] Take 0.0015g of Ni prepared in step (2) of Example 1 1.5 Co 1.5Al1-LDO was added to 30 mL of a 20 mg / L imidacloprid solution, and then 0.0072 g of sodium persulfate (i.e., the concentration of sodium persulfate in the imidacloprid solution was 1 mM) was added, and the reaction was oscillated for 30 min. Samples were taken at 30 min of the catalytic reaction, 1 mL was sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane, and the reaction was terminated. The results showed that the removal rate of imidacloprid was as high as 67%, indicating that the catalyst prepared by the present invention also has a considerable degradation effect on high-concentration neonicotinoid insecticides.

[0097] Example 13

[0098] The application of catalyst in wastewater treatment, its stability and reusability are two important indicators to determine the practical application ability of the catalyst, so this example is Ni 1.5 Co 1.5 The stability and reusability of Al1-LDO are tested. The specific steps are as follows:

[0099] Take the Ni prepared in Example 1 1.5 Co 1.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0071 g of sodium persulfate was added and the reaction was shaken for 30 minutes. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 minutes. 1 mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The used catalyst was washed with deionized water and ethanol and dried, and the above degradation experiment was repeated for a total of 5 cycles. The results are shown in Figure 7 As shown by Figure 7 It can be seen that the Ni provided by the present invention 1.5 Co 1.5 Al1-LDO still maintained its excellent ability to activate persulfate to degrade imidacloprid during the five cycles, and the fifth cycle still had an imidacloprid removal rate of more than 75%.

[0100] Embodiment 14

[0101] In this example, the Ni prepared in Example 1 was tested 1.5 Co 1.5 The degradation ability of Al1-LDO on different neonicotinoid insecticides is as follows:

[0102] Take the Ni prepared in Example 1 1.5 Co 1.5Al1-LDO was added to 30 mL of a 10 mg / L neonicotinoid insecticide solution, with the target pollutants being imidacloprid, thiamethoxam, clothianidin, dinotefuran, nitenpyram, chlorothiazide, and acetamiprid. Then 0.0071 g of sodium persulfate was added and the reaction was shaken for 30 min. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 min, 1 mL was sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in Figure 8 As shown by Figure 8 It can be seen that the Ni provided by the present invention 1.5 Co 1.5 Al1-LDO activated persulfate not only has a high removal capacity for imidacloprid, but also has a good removal capacity for the other 6 neonicotinoid insecticides, and has a good degradation effect on 7 different organic pollutants, most of which can be degraded by more than 80%, indicating that the Ni prepared by the present invention 1.5 Co 1.5 Al1-LDO has excellent removal capabilities for a variety of neonicotinoid pesticides and can be widely used in wastewater treatment of different neonicotinoid pesticides, with broad application prospects.

[0103] Embodiment 15

[0104] In this example, the Ni prepared in Example 1 was tested 1.5 Co 1.5 The degradation ability of Al1-LDO on neonicotinoid insecticides at different pH values ​​is as follows:

[0105] Take the Ni prepared in Example 1 1.5 Co 1.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0071 g of sodium persulfate was added to adjust the pH of each mixed solution to 3, 4, 5, 7, 9, 10, and 12, respectively, and the reaction was oscillated for 30 minutes. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 minutes, 1 mL was sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. The results are shown in Fig. 9 As shown by Fig. 9 It can be seen that the Ni provided by the present invention 1.5 Co 1.5 Al1-LDO activated persulfate has a wide pH applicable range and can efficiently degrade neonicotinoid insecticides in the pH range of 4 to 10.

[0106] Example 16

[0107] In this example, the Ni prepared in Example 1 was tested 1.5 Co 1.5 Al1-LDO contains Cl - , SO4 2- The degradation capacity of neonicotinoid pesticides in water bodies is as follows:

[0108] Take the Ni prepared in Example 1 1.5 Co 1.5 Al1-LDO was added to 30 mL of 10 mg / L imidacloprid solution, and then 0.0071 g of sodium persulfate and a certain amount of NaCl were added to make the Cl in the mixed solution - The concentrations of the mixed solutions were 1mM, 2mM, and 5mM, respectively. In another group of experiments, a certain amount of Na2SO4 was added to make the SO4 2- The concentrations were 1mM, 2mM, and 5mM, and the reaction was oscillated for 30 minutes each. During the catalytic reaction, samples were taken at 3, 5, 8, 15, and 30 minutes. 1 mL of the suspension was sampled and injected into a brown liquid chromatography injection bottle pre-added with 80 μL of methanol through a 0.22 μM organic filter membrane to terminate the reaction. Among them, the degradation effect of imidacloprid in the mixed solution containing NaCl was as follows: Fig.10 As shown in Figure (a), 0mM is the degradation effect of imidacloprid when no NaCl is added. In the mixed solution containing NaSO4, the degradation effect of imidacloprid is as follows Fig.10 As shown in Figure (b), 0 mM in the figure represents the degradation effect of imidacloprid when no NaSO4 is added.

[0109] Depend on Fig.10 It can be seen that in the presence of Cl - , SO4 2- In water, the Ni prepared by the present invention 1.5 Co 1.5 Al1-LDO still has excellent removal ability for neonicotinoid insecticides.

[0110] Embodiment 17

[0111] The preparation steps of flower-shaped NiCoAl layered oxide are as follows:

[0112] (1) 0.015 mol NiCl2, 0.015 mol Co(CH3COO)2, 0.001 mol AlCl3, 0.08 mol urea and 0.004 mol hexadecyltrimethylammonium bromide were added to 100 mL of distilled water in sequence, stirred and mixed, and heated to 60°C for hydrothermal reaction for 16 h, and then a solid product was separated, washed and dried to obtain NiCoAl layered hydroxide, denoted as Ni 15 Co15 Al1-LDH;

[0113] (2) The NiCoAl layered hydroxide obtained in step (1) was heated to 300°C at a heating rate of 2°C / min in an air atmosphere and then kept at that temperature for 2 h. After cooling, NiCoAl layered oxide was obtained, which was denoted as Ni 15 Co 15 Al1-LDO.

[0114] Scanning electron microscopy was used to observe that the Ni 15 Co 15 The morphology of Al1-LDO is also flower ball-shaped and has a high specific surface area.

[0115] Degradation experiment:

[0116] Take 0.015 g of Ni prepared in step (2) of Example 15 15 Co 15 Al1-LDO, added to 30mL of imidacloprid solution with a concentration of 10mg / L, then added 0.0071g of potassium persulfate, and oscillated for 30min. Samples were taken at 3, 5, 8, 15, and 30min during the catalytic reaction, 1mL was sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80μL of methanol through a 0.22μM organic filter membrane to terminate the reaction. In the present embodiment, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 62.5% within 30min.

[0117] Embodiment 18

[0118] The preparation steps of the flower-shaped NiCoAl layered oxide are as follows:

[0119] (1) 0.015 mol Ni(CH3COO)2, 0.015 mol CoCl2, 0.005 mol Al2(SO4)3, 0.1 mol urea and 0.008 mol hexadecyltrimethylammonium bromide were sequentially added into 100 mL distilled water, stirred and mixed, and heated to 160°C for hydrothermal reaction for 6 h, and then a solid product was separated, and the solid product was washed and dried to obtain NiCoAl layered hydroxide, which was recorded as Ni3Co3Al1-LDH;

[0120] (2) The NiCoAl layered hydroxide obtained in step (1) was heated to 600°C at a heating rate of 15°C / min in an air atmosphere and then kept at that temperature for 0.5h. After cooling, a NiCoAl layered oxide was obtained, which was recorded as Ni3Co3Al1-LDO.

[0121] Scanning electron microscope observation revealed that the Ni3Co3Al1-LDO prepared in this example also had a flower ball shape and had a high specific surface area.

[0122] Degradation experiment:

[0123] Take 0.015g of Ni3Co3Al1-LDO prepared in step (2) of embodiment 15, add to 30mL of imidacloprid solution with a concentration of 10mg / L, then add 0.0071g of potassium persulfate, and oscillate for 30min. Samples are taken at the 3rd, 5th, 8th, 15th, and 30min during the catalytic reaction, 1mL is sampled from the suspension, and injected into a brown liquid chromatography injection bottle pre-added with 80μL methanol by a 0.22μM organic filter membrane, and the reaction is terminated. In the present embodiment, the degradation of imidacloprid conforms to the first-order kinetic equation, and the removal rate of imidacloprid reaches 77.2% in 30min.

[0124] The above description is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, and they should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a flower-shaped nickel-cobalt-aluminum layered oxide catalyst, It is characterized in that The following steps are involved: A solution containing nickel salt, cobalt salt, aluminum salt, alkaline substance and template agent is stirred and subjected to hydrothermal reaction, and the obtained solid nickel-cobalt-aluminum layered hydroxide is calcined to obtain the flower-spherical nickel-cobalt-aluminum layered oxide catalyst; The alkaline substance is urea and / or ammonia water, and the template agent is hexadecyltrimethylammonium bromide; In the solution, the concentration of nickel salt is 0.025-0.25 mol / L, the concentration of cobalt salt is 0.025-0.25 mol / L, and the concentration of aluminum salt is 0.01-0.1 mol / L; in the solution, the molar ratio of nickel salt, cobalt salt and aluminum salt is (0.1-3):(0.1-3):1; and the concentration of template agent is 0.01-0.1 mol / L.

2. The method for preparing the flower-spherical nickel-cobalt-aluminum layered oxide catalyst according to claim 1, It is characterized in that The nickel salt includes NiCl 2 ,Ni(NO 3 ) 2 and Ni(CH 3 COO 2 At least one of the cobalt salts comprising CoCl 2 、Co(NO 3 ) 2 and Co(CH 3 COO 2 At least one of the following, wherein the aluminum salt comprises AlCl 3 、Al(NO 3 ) 3 and Al 2 (SO 4 ) 3 At least one of .

3. The method for preparing the flower-spherical nickel-cobalt-aluminum layered oxide catalyst according to claim 1, It is characterized in that In the solution, the concentration of the alkaline substance is 0.12-1.2 mol / L.

4. The method for preparing the flower-spherical nickel-cobalt-aluminum layered oxide catalyst according to claim 1, It is characterized in that The hydrothermal temperature is 60-160° C., and the reaction time is 6-16 hours; the calcination temperature is 300-600° C., and the time is 0.5-2 hours.

5. A flower-spherical nickel-cobalt-aluminum layered oxide catalyst prepared according to the method for preparing a flower-spherical nickel-cobalt-aluminum layered oxide catalyst according to any one of claims 1 to 4.

6. Use of the flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst according to claim 5 in degrading neonicotinoid pesticides in water, It is characterized in that The following steps are involved: The flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst and persulfate are added to water containing neonicotinoid pesticides to react, thereby completing the degradation treatment of the neonicotinoid pesticides in the water.

7. The use according to claim 6, It is characterized in that In the water containing neonicotinoid insecticides, the concentration of neonicotinoid insecticides is 1-20 mg / L, the concentration of the flower ball-shaped nickel-cobalt-aluminum layered oxide catalyst is 0.1-1.5 g / L, and the concentration of persulfate is 0.5-5 mM; and the reaction time is 0.5 h.

8. The use according to claim 6, It is characterized in that The persulfate includes at least one of sodium persulfate, potassium persulfate, sodium permonosulfate, potassium permonosulfate and potassium hydrogen persulfate.