A kind of bending and wear-resistant colorful TPU film and its preparation method and application

By using polyester acrylate and other materials in the TPU film and composite fillers of tungsten carbide, copper oxide, and graphite, combined with UV curing and electron beam evaporation or magnetron sputtering technology, the problem of insufficient resistance to tortuous and wear resistance of TPU film is solved. , significantly improves the film's folding and wear resistance.

CN117924778BActive Publication Date: 2024-11-08DONGGUAN QUANFENG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410119463.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2024-11-08
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

Existing TPU films are prone to cracks and fractures during frequent folding, extrusion and bending operations, resulting in insufficient resistance to torsion and wear resistance, affecting the service life and quality of the product.

Method used

A colorful TPU film consisting of a TPU bare mold layer, an adhesive layer and an electroplating layer is used. The adhesive layer is composed of polyester acrylate oligomer, aliphatic polyurethane acrylate, tetrahydrofuran acrylate and other materials, and carbonization is added. Tungsten, copper oxide and graphite composite fillers are prepared by UV curing and electron beam evaporation or magnetron sputtering technology to enhance the film's torsion and wear resistance.

Benefits of technology

It improves the torsion resistance and wear resistance of the TPU film, extends the service life of the product, and enhances the user experience.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a tortuosity-resistant and wear-resistant colorful TPU film and its preparation method and application, belonging to the technical field of TPU films. The colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer in order from bottom to top. The adhesive layer is made by printing an adhesive on the surface of the TPU bare mold layer and UV curing. The preparation method of the adhesive comprises the following steps: S1, temperature-controlled mixing of polyester acrylate oligomer, aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, active diluent and glycidyl ether epoxyphenyl siloxane to obtain a mixture A; S2, adding a leveling agent and a photoinitiator to the mixture A and stirring at a controlled temperature to obtain a mixture B; S3, adding a composite filler and phosphorylated nanocellulose to the mixture B and stirring to obtain an adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of TPU films, and in particular, relates to a bending-resistant and wear-resistant colorful TPU film and a preparation method and application thereof. Background Art

[0002] TPU film is a thermoplastic polyurethane film with the characteristics of high strength, high elasticity, high transparency and chemical resistance. The TPU film sold on the market is usually not just a bare mold layer, but a TPU film composed of a bare mold layer, a glue layer and an electroplating layer. For the sake of beauty, many merchants will also use different atmospheres when preparing the electroplating layer to prepare an electroplating layer with a dazzling visual effect to enhance the appearance of the product. Therefore, its unique material properties make TPU film widely used in the fields of bag film, handbag film, decorative film and label film. In actual application, products such as handbag film and label film usually need to withstand frequent folding, extrusion and bending operations. If the film material does not have good bending resistance and wear resistance, it will easily cause cracks, fractures and other problems, reducing the service life and quality of the product. Therefore, in order to solve the above problems, it is particularly important to provide a TPU film with good bending resistance and wear resistance, which can improve the quality and performance of the product and enhance the user experience. Summary of the invention

[0003] The purpose of the present invention is to provide a colorful TPU film that is resistant to bending and wear, and a preparation method and application thereof. The colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer from bottom to top. The adhesive layer is made by printing the adhesive on the surface of the TPU bare mold layer and UV curing. Among the raw materials of the adhesive, polyester acrylate oligomer and aliphatic polyurethane acrylate are used as the main resins, and trimethylolpropane triacrylate is used to increase the crosslinking density of the system. At the same time, tetrahydrofuran acrylate is used to assist in reducing the rigidity of the polymer, so that the finished product has good bending resistance; and the composite filler composed of tungsten carbide, copper oxide and graphite cooperates to make the finished product have excellent wear resistance; solving the problem of poor bending resistance and wear resistance of TPU film in the prior art.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A colorful TPU film that is resistant to bending and wear, wherein the colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer in sequence from bottom to top.

[0006] A method for preparing a colorful TPU film that is resistant to bending and wear, the preparation method comprising the following steps:

[0007] A1, melt-extrude TPU particles and blow-form them into films to obtain a TPU bare mold layer;

[0008] A2, printing adhesive on the surface of the TPU bare mold layer, UV curing, to obtain an adhesive layer;

[0009] A3. A metal layer is plated on the surface of the adhesive layer by electron beam evaporation or magnetron sputtering to obtain an electroplated layer.

[0010] As a preferred technical solution of the present invention, the thickness of the TPU bare mold layer in step A1 is 0.1-0.15 mm.

[0011] As a preferred technical solution of the present invention, the thickness of the adhesive layer in step A2 is 20-25 μm.

[0012] As a preferred technical solution of the present invention, the wavelength of UV curing in step A2 is 365-395nm.

[0013] As a preferred technical solution of the present invention, the preparation method of the adhesive in step A2 comprises the following steps:

[0014] S1, mixing polyester acrylate oligomer, aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane uniformly under temperature control to obtain a mixture A;

[0015] S2, adding a leveling agent and a photoinitiator to mixed material A and stirring under controlled temperature to obtain mixed material B;

[0016] S3. Add the composite filler and phosphorylated nanocellulose into the mixture B and stir to obtain an adhesive.

[0017] As a preferred technical solution of the present invention, the mass ratio of the polyester acrylate oligomer, aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane in step S1 is 30-32:18-20:13-15:16-18:10-11:6-7.

[0018] As a preferred technical solution of the present invention, the temperature for temperature-controlled mixing in step S1 is 35-40°C.

[0019] As a preferred technical solution of the present invention, the aliphatic polyurethane acrylate in step S1 is monofunctional or difunctional.

[0020] As a preferred technical solution of the present invention, the active diluent in step S1 is composed of 2,3-epoxypropyl methacrylate and 1,6-hexanediol diacrylate in an equal mass ratio.

[0021] As a preferred technical solution of the present invention, the mass ratio of the mixed material A, the leveling agent and the photoinitiator in step S2 is 1:2-2.5:3-3.5.

[0022] As a preferred technical solution of the present invention, the temperature of the temperature-controlled stirring in step S2 is 50-55° C. and the time is 1-2 h.

[0023] As a preferred technical solution of the present invention, the leveling agent in step S2 includes BYK354 and CAB-551-0.2 in a mass ratio of 0.2-0.3:1.7.

[0024] As a preferred technical solution of the present invention, the photoinitiator in step S2 is lrgacure184.

[0025] As a preferred technical solution of the present invention, the mass ratio of the mixture B, the composite filler and the phosphorylated nanocellulose in step S3 is 1:5-6:0.04-0.05.

[0026] As a preferred technical solution of the present invention, the composite filler includes tungsten carbide, copper oxide and graphite.

[0027] As a preferred technical solution of the present invention, the mass ratio of tungsten carbide, copper oxide and graphite is 1:0.7-0.8:1-1.2.

[0028] As a preferred technical solution of the present invention, the stirring time in step S3 is 20-30 minutes.

[0029] As a preferred technical solution of the present invention, the polyester acrylate polymer used in the embodiments and comparative examples of the present invention was purchased from Shanghai Chemelite Chemical Technology Co., Ltd. with the brand name CN966J75NS; the glycidyl ether epoxyphenyl siloxane model number is EPPh2, purchased from Dongguan Weizhimei New Material Technology Co., Ltd.; the phosphorylated nanocellulose was purchased from Xi'an Qiyue Biotechnology Co., Ltd.

[0030] As a preferred technical solution of the present invention, the thickness of the electroplating layer in step A3 is 18-20 μm.

[0031] As a preferred technical solution of the present invention, the current for plating a metal layer in step A3 is 20-100A and the time is 1 min; the atmosphere for plating a metal layer is argon atmosphere or nitrogen atmosphere; when argon atmosphere is selected, the coating has a metallic color effect, and when nitrogen atmosphere is selected, the coating has a colorful effect.

[0032] An application of a colorful TPU film that is resistant to bending and abrasion, including but not limited to making the colorful TPU film into bag film, handbag film, decorative film, label film, etc.

[0033] Beneficial effects of the present invention:

[0034] (1) The present invention uses polyester acrylate copolymers with excellent compatibility and low viscosity and aliphatic polyurethane acrylate with fast curing and good chemical stability as the main resins, and trimethylolpropane triacrylate is used to increase the crosslinking density of the system to improve the flexibility of the finished product. At the same time, tetrahydrofuran acrylate with a low glass transition temperature is used to assist in reducing the rigidity of the polymer, further improving the flexibility of the obtained adhesive layer, so that the finished product has better bending resistance.

[0035] (2) The present invention adds a composite filler composed of tungsten carbide, copper oxide and graphite, with tungsten carbide and copper oxide playing the main role of anti-friction and load bearing, and graphite playing a lubricating role to improve the lubricity of tungsten carbide and copper oxide. The three work together to solve the problem that a single filler is difficult to improve the wear resistance of the system. On this basis, the hydrophilic hydroxyl groups on the surface of phosphorylated nanocellulose interact with the composite filler to prevent the composite filler from agglomerating in the system, thereby achieving uniform dispersion in the system and further enhancing the wear resistance of the finished product.

[0036] (3) The present invention adds glycidyl ether epoxyphenyl siloxane containing silicon-oxygen bonds and hydrocarbon groups in the molecular chain. When it is heat-aged, it can form a protective layer rich in silicon-oxygen bond molecular chains on the surface, reducing the impact on the interior of the polymer and effectively increasing the thermal stability of the finished product. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] A colorful TPU film that is resistant to bending and abrasion, wherein the colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer in order from bottom to top;

[0040] The method for preparing the bending-resistant and wear-resistant colorful TPU film comprises the following steps:

[0041] A1. Melt-extrude and blow-form TPU particles into films to obtain a TPU bare mold layer; the TPU bare mold layer has a thickness of 0.1 mm;

[0042] A2, embossing adhesive on the surface of the TPU bare mold layer, and UV curing at a wavelength of 395nm after embossing to obtain an adhesive layer, that is, obtaining a semi-finished product of embossing adhesive on the TPU bare mold layer; the thickness of the adhesive layer is 25μm;

[0043] A3. A metal layer is plated on the surface of the adhesive layer by electron beam evaporation to obtain an electroplated layer, that is, a colorful TPU film finished product with an electroplated layer on the semi-finished product is obtained; the thickness of the electroplated layer is 18 μm; the current for plating the metal layer is 20 A, and the plating time is 1 min; the atmosphere for plating the metal layer is an argon atmosphere.

[0044] The preparation method of the adhesive in step A2 comprises the following steps:

[0045] S1. Polyester acrylate oligomer, difunctional aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane are mixed uniformly at a mass ratio of 30:18:14:18:11:6 and the temperature is controlled at 35° C. to obtain a mixture A;

[0046] The active diluent is composed of 2,3-epoxypropyl methacrylate and 1,6-hexanediol diacrylate in an equal mass ratio;

[0047] S2. Add leveling agent and lrgacure184 to mixed material A and stir at 50°C for 1.5h to obtain mixed material B;

[0048] The mass ratio of the mixture A, the leveling agent and lrgacure184 is 1:2:3.5;

[0049] The leveling agent includes BYK354 and CAB-551-0.2 in a mass ratio of 0.2:1.7;

[0050] S3, adding composite filler and phosphorylated nanocellulose to mixture B and stirring for 30 minutes to obtain an adhesive;

[0051] The mass ratio of the mixture B, the composite filler and the phosphorylated nanocellulose is 1:6:0.04;

[0052] The composite filler comprises tungsten carbide, copper oxide and graphite in a mass ratio of 1:0.7:1.2.

[0053] Example 2

[0054] A colorful TPU film that is resistant to bending and abrasion, wherein the colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer in order from bottom to top;

[0055] The method for preparing the bending-resistant and wear-resistant colorful TPU film comprises the following steps:

[0056] A1. Melt-extrude and blow-mold TPU particles into films to obtain a TPU bare mold layer; the TPU bare mold layer has a thickness of 0.15 mm;

[0057] A2, embossing adhesive on the surface of the TPU bare mold layer, and UV curing at a wavelength of 365nm after embossing to obtain an adhesive layer, that is, a semi-finished product of embossing adhesive on the TPU bare mold layer is obtained; the thickness of the adhesive layer is 20μm;

[0058] A3. A metal layer is plated on the surface of the adhesive layer by magnetron sputtering to obtain an electroplated layer, that is, a colorful TPU film finished product with an electroplated layer on the semi-finished product is obtained; the thickness of the electroplated layer is 20 μm; the current for plating the metal layer is 100 A, and the plating time is 1 min; the atmosphere for plating the metal layer is a nitrogen atmosphere.

[0059] The preparation method of the adhesive in step A2 comprises the following steps:

[0060] S1. Polyester acrylate oligomer, difunctional aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane are mixed uniformly at a mass ratio of 32:19:13:16:10.5:6.5 at a temperature of 40° C. to obtain a mixture A;

[0061] The active diluent is composed of 2,3-epoxypropyl methacrylate and 1,6-hexanediol diacrylate in an equal mass ratio;

[0062] S2. Add leveling agent and lrgacure184 to mixed material A and stir at 55°C for 1.5h to obtain mixed material B;

[0063] The mass ratio of the mixture A, the leveling agent and lrgacure184 is 1:2.5:3;

[0064] The leveling agent comprises BYK354 and CAB-551-0.2 in a mass ratio of 0.25:1.7;

[0065] S3, adding composite filler and phosphorylated nanocellulose to mixture B and stirring for 20 minutes to obtain an adhesive;

[0066] The mass ratio of the mixture B, the composite filler and the phosphorylated nanocellulose is 1:5:0.05;

[0067] The composite filler comprises tungsten carbide, copper oxide and graphite in a mass ratio of 1:0.75:1.1.

[0068] Example 3

[0069] A colorful TPU film that is resistant to bending and abrasion, wherein the colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer in order from bottom to top;

[0070] The method for preparing the bending-resistant and wear-resistant colorful TPU film comprises the following steps:

[0071] A1. Melt-extrude and blow-mold TPU particles into films to obtain a TPU bare mold layer; the TPU bare mold layer has a thickness of 0.13 mm;

[0072] A2, embossing adhesive on the surface of the TPU bare mold layer, and UV curing at a wavelength of 380nm after embossing to obtain an adhesive layer, that is, obtaining a semi-finished product of embossing adhesive on the TPU bare mold layer; the thickness of the adhesive layer is 23μm;

[0073] A3. A metal layer is plated on the surface of the adhesive layer by magnetron sputtering to obtain an electroplated layer, that is, a colorful TPU film finished product with an electroplated layer on the semi-finished product is obtained; the thickness of the electroplated layer is 19 μm; the current for plating the metal layer is 60 A, and the plating time is 1 min; the atmosphere for plating the metal layer is an argon atmosphere.

[0074] The preparation method of the adhesive in step A2 comprises the following steps:

[0075] S1. Polyester acrylate oligomer, monofunctional aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane are mixed uniformly at a mass ratio of 31:20:15:17:10:7 and the temperature is controlled at 38° C. to obtain a mixture A;

[0076] The active diluent is composed of 2,3-epoxypropyl methacrylate and 1,6-hexanediol diacrylate in an equal mass ratio;

[0077] S2. Add leveling agent and lrgacure184 to mixed material A and stir at 53°C for 1 hour to obtain mixed material B;

[0078] The mass ratio of the mixture A, the leveling agent and lrgacure184 is 1:2.3:3.3;

[0079] The leveling agent includes BYK354 and CAB-551-0.2 in a mass ratio of 0.3:1.7;

[0080] S3, adding composite filler and phosphorylated nanocellulose to mixture B and stirring for 25 minutes to obtain an adhesive;

[0081] The mass ratio of the mixture B, the composite filler and the phosphorylated nanocellulose is 1:5.5:0.04;

[0082] The composite filler comprises tungsten carbide, copper oxide and graphite in a mass ratio of 1:0.8:1.

[0083] Comparative Example 1

[0084] Compared with Example 3, the difference is that trimethylolpropane triacrylate is not added in Comparative Example 1, and the other parameters and operation steps remain unchanged.

[0085] Comparative Example 2

[0086] Compared with Example 3, the difference is that tetrahydrofuran acrylate is not added in Comparative Example 2, and the other parameters and operating steps remain unchanged.

[0087] Comparative Example 3

[0088] Compared with Example 3, the difference is that the composite filler of Comparative Example 3 includes copper oxide and graphite in a mass ratio of 1.3:1.5, and the other parameters and operating steps remain unchanged.

[0089] Comparative Example 4

[0090] Compared with Example 3, the difference is that the composite filler of Comparative Example 4 is composed of tungsten carbide and graphite in a mass ratio of 1.4:1.4, and the other parameters and operating steps remain unchanged.

[0091] Comparative Example 5

[0092] Compared with Example 3, the difference is that the composite filler of Comparative Example 5 is composed of tungsten carbide and copper oxide in a mass ratio of 1.5:1.3, and the other parameters and operating steps remain unchanged.

[0093] Comparative Example 6

[0094] Compared with Example 3, the difference is that in Comparative Example 6, phosphorylated nanocellulose is not added, and the other parameters and operating steps remain unchanged.

[0095] Comparative Example 7

[0096] Compared with Example 3, the difference is that in Comparative Example 7, no glycidyl ether epoxyphenyl siloxane is added, and the other parameters and operating steps remain unchanged.

[0097] Test Case

[0098] (1) Bend resistance test: The semi-finished products obtained in step A2 of Example 1-3 and Comparative Example 1-2 were cut into a size of 70 mm × 45 mm. The semi-finished products were subjected to a 50,000-fold bending test at room temperature with the same test parameters using a folding resistance tester. The surface damage of the adhesive layer of the semi-finished products after the bending test was observed. The test results are shown in Table 1.

[0099] (2) Vibration wear resistance test: The semi-finished products obtained in step A2 of Examples 1-3 and Comparative Examples 3-6 were placed in a vibration wear resistance machine for 2 h. The adhesive layer of the semi-finished products was subjected to a vibration wear resistance test with the same test parameters. The appearance of the adhesive layer of the semi-finished products after the test was observed to determine if they fell off. The test results are shown in Table 1.

[0100] (3) Thermal stability test: The semi-finished products obtained in step A2 of Examples 1-3 and Comparative Example 7 were cut into sheets of 20 cm × 20 cm in size and placed in an oven at 180° C. for 30 min. The adhesive layer on the surface of the semi-finished products was observed to see if there was any separation or falling off. The test results are shown in Table 1.

[0101] Table 1

[0102] Resistance to bending Vibration wear resistance Thermal stability Example 1 No damage qualified No separation or falling off Example 2 No damage qualified No separation or falling off Example 3 No damage qualified No separation or falling off Comparative Example 1 Visible damage —— —— Comparative Example 2 Slightly damaged —— —— Comparative Example 3 —— Obvious shedding —— Comparative Example 4 —— Obvious shedding —— Comparative Example 5 —— Slight shedding —— Comparative Example 6 —— Slight shedding —— Comparative Example 7 —— —— Large area separation and small part falling off

[0103] It can be seen from the data of Examples 1-3 and Comparative Examples 1-2 in Table 1 that the trimethylolpropane triacrylate and tetrahydrofuran acrylate added in the present invention can effectively make the finished product have excellent flexural resistance;

[0104] It can be seen from the data of Examples 1-3 and Comparative Examples 3-6 that if any one of the composite fillers or phosphorylated nanocellulose is not added, the vibration wear resistance of the finished product is poor. Obviously, the composite fillers composed of tungsten carbide, copper oxide and graphite can synergistically solve the problem that a single filler is difficult to improve the wear resistance of the system;

[0105] It can be seen from the data of Examples 1-3 and Comparative Example 7 that the glycidyl ether epoxyphenyl siloxane added in the present invention can effectively increase the thermal stability of the finished product.

[0106] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0107] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A colorful TPU film that is resistant to bending and wear, characterized in that: The colorful TPU film is composed of a TPU bare mold layer, an adhesive layer and an electroplating layer from bottom to top; The method for preparing the bending-resistant and wear-resistant colorful TPU film comprises the following steps: A1, melt-extrude TPU particles and blow-form them into films to obtain a TPU bare mold layer; A2, printing adhesive on the surface of the TPU bare mold layer, UV curing, to obtain an adhesive layer; A3, coating a metal layer on the surface of the adhesive layer by electron beam evaporation or magnetron sputtering to obtain an electroplated layer; The preparation method of the adhesive described in step A2 comprises the following steps: S1, mixing polyester acrylate oligomer, aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane uniformly under temperature control to obtain a mixture A; S2, adding a leveling agent and a photoinitiator to mixed material A and stirring under controlled temperature to obtain mixed material B; S3. Add the composite filler and phosphorylated nanocellulose into the mixture B and stir to obtain an adhesive.

2. The flexure-resistant and wear-resistant colorful TPU film according to claim 1, characterized in that: In step S1, the mass ratio of the polyester acrylate oligomer, aliphatic polyurethane acrylate, tetrahydrofuran acrylate, trimethylolpropane triacrylate, reactive diluent and glycidyl ether epoxyphenyl siloxane is 30-32:18-20:13-15:16-18:10-11:6-7.

3. The flexure-resistant and wear-resistant colorful TPU film according to claim 1, characterized in that: The active diluent in step S1 is composed of 2,3-epoxypropyl methacrylate and 1,6-hexanediol diacrylate in an equal mass ratio.

4. The flexure-resistant and wear-resistant colorful TPU film according to claim 1, characterized in that: The mass ratio of the mixed material A, the leveling agent and the photoinitiator in step S2 is 1:2-2.5:3-3.

5.

5. The flexure-resistant and wear-resistant colorful TPU film according to claim 1, characterized in that: The leveling agent in step S2 includes BYK354 and CAB-551-0.2 in a mass ratio of 0.2-0.3:1.

7.

6. The flexure-resistant and wear-resistant colorful TPU film according to claim 1, characterized in that: In step S3, the mass ratio of the mixture B, the composite filler and the phosphorylated nanocellulose is 1:5-6:0.04-0.

05.

7. The flexure-resistant and wear-resistant colorful TPU film according to claim 6, characterized in that: The composite filler includes tungsten carbide, copper oxide and graphite.

8. The flexure-resistant and wear-resistant colorful TPU film according to claim 7, characterized in that: The mass ratio of the tungsten carbide, copper oxide and graphite is 1:0.7-0.8:1-1.2.

Citation Information

Cited By

  • High-tensile matte colorful TPU (thermoplastic polyurethane) film and preparation method thereof