Polyurethane coating composition and application thereof, polyurethane coating and preparation method thereof

By using specific compositions and processes in polyurethane coatings, the problem of bubbles produced by traditional polyurethane coatings during moisture curing is solved, its mechanical properties and stability are significantly improved, and bubble-free and high-performance coatings are achieved. .

CN117946582BActive Publication Date: 2024-10-29福建科顺新材料有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311798906.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-10-29
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

Traditional one-component polyurethane coatings are prone to bubbles during the moisture curing process, which affects their storage stability and mechanical properties. It is difficult to effectively solve the problems of poor defoaming effect and low coating film performance with existing technology.

Method used

Using a composition containing diisocyanate, polyether polyol, powder filler, plasticizer, first auxiliary agent, second auxiliary agent and solvent, through specific proportions and process processing, a bubble-free polyurethane coating is prepared, which improves the Its mechanical properties and performance retention rate.

Benefits of technology

It achieves the bubble-free characteristics and excellent mechanical property retention rate of polyurethane coatings, improving the stability and performance of the coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004628396890000021
    Figure BDA0004628396890000021
  • Figure BDA0004628396890000031
    Figure BDA0004628396890000031
  • Figure BDA0004628396890000041
    Figure BDA0004628396890000041
Patent Text Reader

Abstract

The present invention relates to the field of waterproof coatings, and discloses a polyurethane coating composition and its application, a polyurethane coating and its preparation method. The polyurethane coating composition comprises the following components: diisocyanate, polyether polyol, powder filler, plasticizer, first auxiliary agent, second auxiliary agent and solvent; the second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate. The polyurethane waterproof coating of the present invention has the characteristic of no bubbles, and has excellent mechanical properties and mechanical property retention rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waterproof coatings, and in particular to a polyurethane coating composition and application thereof, a polyurethane coating and a preparation method thereof. Background Art

[0002] The principle of traditional single-component polyurethane is moisture curing. The -NCO in the polyurethane material directly reacts with water in the air, and the molecular chain segments grow to cross-link and cure. Curing can be achieved with only a trace amount of water in the air. It has the advantages of simple process and low curing cost.

[0003] However, traditional one-component polyurethane will also release carbon dioxide during moisture curing. The generated carbon dioxide will produce bubbles or pinholes in the film, thereby affecting the physical properties of the polyurethane waterproof coating. During storage and use, problems such as foaming and bubbling often occur, affecting the storage stability of the one-component polyurethane and reducing the mechanical properties of the material.

[0004] CN107936647A discloses a scratch-resistant water-based polyurethane coating, comprising silicone-acrylic emulsion, epoxy polyurethane latex, heptadecafluorodecyl methacrylate, curing agent, neopentyl glycol, silicone, cyclohexanone, glass powder, and initiator. The polyurethane coating prepared by this technical solution solves the problem of poor ductility of the coating film, but cannot solve the problem that -NCO easily reacts with moisture to produce bubbles.

[0005] CN104845518 discloses a polyurethane waterproof coating. Through the reasonable proportion of the raw materials of the invention, the prepared polyurethane coating has the advantages of wide applicability, high strength, large elongation, good elasticity and good waterproof effect. However, the prior art cannot solve the problems of foaming and blistering of the polyurethane coating in a high humidity environment.

[0006] At present, it is of great significance to solve the problems of poor defoaming effect and low coating performance of polyurethane coatings. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of the polyurethane waterproof coating in the prior art, such as poor defoaming effect and low coating film performance.

[0008] In order to achieve the above object, the first aspect of the present invention provides a polyurethane coating composition, which contains the following components stored separately or in a mixture of two or more:

[0009] Diisocyanate, polyether polyol, powder filler, plasticizer, first auxiliary agent, second auxiliary agent and solvent;

[0010] Based on the total weight of the coating, the content of the diisocyanate is 3-8wt%, the content of the polyether polyol is 20-40wt%, the content of the powder filler is 30-40wt%, the content of the plasticizer is 10-20wt%, the content of the first auxiliary agent is 2-6wt%, the content of the second auxiliary agent is 0.2-1.5wt%, and the content of the solvent is 4-15wt%;

[0011] The polyether polyol has a hydroxyl value of 36-58 mgKOH / g and an acid value of ≤0.5 mgKOH / g;

[0012] The first auxiliary agent is a structure shown in formula (I),

[0013]

[0014] The second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate.

[0015] The second aspect of the present invention provides use of the composition described in the first aspect in a polyurethane coating.

[0016] The third aspect of the present invention provides a method for preparing a polyurethane coating, the method comprising: mixing and contacting the components in a composition containing a diisocyanate, a polyether polyol, a powder filler, a plasticizer, a first auxiliary agent, a second auxiliary agent and a solvent to obtain the polyurethane coating;

[0017] Based on the total amount of the composition, the amount of the diisocyanate is 3-8wt%, the amount of the polyether polyol is 20-40wt%, the amount of the powder filler is 30-40wt%, the amount of the plasticizer is 10-20wt%, the amount of the first auxiliary agent is 2-6wt%, the amount of the second auxiliary agent is 0.2-1.5wt%, and the amount of the solvent is 4-15wt%;

[0018] The polyether polyol has a hydroxyl value of 36-58 mgKOH / g and an acid value of ≤0.5 mgKOH / g;

[0019] The first auxiliary agent is a structure shown in formula (I),

[0020]

[0021] The second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate;

[0022] The composition is the polyurethane coating composition described in the first aspect.

[0023] The fourth aspect of the present invention provides a polyurethane coating prepared by the method described in the third aspect.

[0024] Compared with the prior art, the present invention has at least the following advantages:

[0025] The polyurethane waterproof coating prepared by the technical solution provided by the present invention has the characteristic of being free of bubbles, and has excellent mechanical properties and mechanical property retention rate. DETAILED DESCRIPTION

[0026] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0027] As mentioned above, the first aspect of the present invention provides a polyurethane coating composition, which contains the following components stored separately or in a mixture of two or more:

[0028] Diisocyanate, polyether polyol, powder filler, plasticizer, first auxiliary agent, second auxiliary agent and solvent;

[0029] Based on the total weight of the coating, the content of the diisocyanate is 3-8wt%, the content of the polyether polyol is 20-40wt%, the content of the powder filler is 30-40wt%, the content of the plasticizer is 10-20wt%, the content of the first auxiliary agent is 2-6wt%, the content of the second auxiliary agent is 0.2-1.5wt%, and the content of the solvent is 4-15wt%;

[0030] The polyether polyol has a hydroxyl value of 36-58 mgKOH / g and an acid value of ≤0.5 mgKOH / g;

[0031] The first auxiliary agent is a structure shown in formula (I),

[0032]

[0033] The second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate.

[0034] Preferably, the first auxiliary agent is a product prepared by the following method, which comprises:

[0035] In the presence of an organic solvent, 2-methyl-1,5-pentanediamine and benzaldehyde are contacted and mixed, and the product obtained after the contact and mixing is subjected to reduced pressure distillation to obtain an auxiliary material as the first auxiliary agent;

[0036] More preferably, the weight ratio of the benzaldehyde to the 2-methyl-1,5-pentanediamine is 1:0.2-0.40, and the amount of the organic solvent is 2-4 mL for every 1 g of the benzaldehyde.

[0037] Preferably, the organic solvent is cyclohexane.

[0038] Further preferably, the contact mixing conditions include: temperature of 45-65° C. and time of 5.5-6.5 h.

[0039] Preferably, the conditions of the reduced pressure distillation treatment include: a temperature of 40-55° C. and a pressure of 0.1-0.5 MPa.

[0040] Preferably, the diisocyanate is selected from at least one of toluene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate. The inventors of the present invention have found that under this preferred condition, the polyurethane coating of the present invention has a better bubble-free effect, better mechanical properties and better mechanical property retention rate.

[0041] More preferably, the polyether polyol is selected from at least one of polyether polyol 2000 and polyether polyol 3000. The inventors of the present invention have found that under this preferred condition, the polyurethane coating of the present invention has better bubble-free effect, better mechanical properties and mechanical property retention rate.

[0042] Preferably, the powder filler is selected from at least one of titanium dioxide, heavy calcium powder and talcum powder.

[0043] Preferably, the average particle size of the powder filler is 2.6 μm-6.5 μm.

[0044] Further preferably, the plasticizer is selected from at least one of chlorinated paraffin, diisononyl phthalate and dioctyl phthalate.

[0045] Preferably, the solvent is selected from at least one of 1,2,4-trimethylbenzene and 1,2,4,5-tetramethylbenzene.

[0046] As mentioned above, the second aspect of the present invention provides the use of the composition described in the first aspect in a polyurethane coating.

[0047] As mentioned above, the third aspect of the present invention provides a method for preparing a polyurethane coating, the method comprising: mixing and contacting the components in a composition containing a diisocyanate, a polyether polyol, a powder filler, a plasticizer, a first auxiliary agent, a second auxiliary agent and a solvent to obtain the polyurethane coating;

[0048] Based on the total amount of the composition, the amount of the diisocyanate is 3-8wt%, the amount of the polyether polyol is 20-40wt%, the amount of the powder filler is 30-40wt%, the amount of the plasticizer is 10-20wt%, the amount of the first auxiliary agent is 2-6wt%, the amount of the second auxiliary agent is 0.2-1.5wt%, and the amount of the solvent is 4-15wt%;

[0049] The polyether polyol has a hydroxyl value of 36-58 mgKOH / g and an acid value of ≤0.5 mgKOH / g;

[0050] The first auxiliary agent is a structure shown in formula (I),

[0051]

[0052] The second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate;

[0053] The composition is the polyurethane coating composition described in the first aspect.

[0054] The types and dosages of the substances involved in the third aspect of the present invention are the same as the types and contents involved in the composition of the first aspect of the present invention. In order to avoid redundancy, the present invention will not be repeated in the third aspect, and those skilled in the art should not understand it as a limitation of the present invention.

[0055] According to a preferred embodiment, the step of mixed contact treatment comprises:

[0056] (1) subjecting a polyether polyol to a first reaction with a plasticizer to obtain a material A;

[0057] (2) subjecting the material A to a second reaction with a powder filler to obtain a material B;

[0058] (3) subjecting the material B to a third reaction with diisocyanate to obtain material C;

[0059] (4) subjecting the material C to a fourth reaction with the first auxiliary agent, the second auxiliary agent and the solvent to obtain the polyurethane coating.

[0060] Preferably, in step (1), the conditions of the first reaction include: temperature of 70-90° C., stirring speed of 300-400 rpm, and stirring time of 0.3-0.8 h.

[0061] Further preferably, in step (2), the conditions of the second reaction include: temperature of 100-120° C., stirring speed of 1100-1300 rpm, and stirring time of 0.3-0.8 h.

[0062] Preferably, in step (3), the conditions of the third reaction include: temperature of 40-60° C., stirring speed of 450-550 rpm, and stirring time of 1.5-2.5 h.

[0063] Preferably, in step (4), the conditions of the fourth reaction include: the vacuum degassing time is 40-50 min; the vacuum degassing pressure is -0.095 MPa to -0.1 MPa.

[0064] According to another specific preferred embodiment, the method comprises:

[0065] (S1) preparing an auxiliary material as the first auxiliary agent:

[0066] In the presence of an organic solvent, 2-methyl-1,5-pentanediamine and benzaldehyde are contacted and mixed, and the product obtained after the contact and mixing is subjected to reduced pressure distillation to obtain an auxiliary material as the first auxiliary agent;

[0067] (S2) subjecting the polyether polyol to a first reaction with a plasticizer to obtain material A;

[0068] (S3) subjecting the material A to a second reaction with a powder filler to obtain a material B;

[0069] (S4) subjecting the material B to a third reaction with diisocyanate to obtain material C;

[0070] (S5) subjecting the material C to a fourth reaction with the auxiliary material, the second auxiliary agent and the solvent obtained in step (S1) to obtain the polyurethane coating. The inventors of the present invention have found that under this preferred condition, the polyurethane coating of the present invention has a better bubble-free effect, better mechanical properties and better mechanical property retention rate.

[0071] The step (S1) involved in the third aspect of the present invention is the same as the method for preparing the first auxiliary agent in the first aspect of the present invention; the steps (S2), (S3), (S4) and (S5) involved in the third aspect of the present invention are the same as the corresponding steps (1), (2), (3) and (4) in the above text. In order to avoid redundancy, the present invention will not be repeated in the rest of the third aspect, and those skilled in the art should not be understood as limiting the present invention.

[0072] Preferably, in step (S2), the conditions of the first reaction include: temperature of 70-90°C, stirring speed of 300-400 rpm, and stirring time of 0.3-0.8h.

[0073] Further preferably, in step (S3), the conditions of the second reaction include: temperature of 100-120° C., stirring speed of 1100-1300 rpm, and stirring time of 0.3-0.8 h.

[0074] Preferably, in step (S3), a vacuum dehydration step is further included after the second reaction, and the conditions of the vacuum dehydration include: vacuum pressure of -0.095MPa to -0.1MPa, and time of 3.5-4.5h.

[0075] Preferably, in step (S4), the conditions of the third reaction include: temperature of 40-60° C., stirring speed of 450-550 rpm, and stirring time of 1.5-2.5 h.

[0076] Further preferably, in step (S5), the conditions of the fourth reaction include: the vacuum degassing time is 40-50 min; the vacuum degassing pressure is -0.095 MPa to -0.1 MPa.

[0077] As mentioned above, the fourth aspect of the present invention provides a polyurethane coating prepared by the method described in the third aspect.

[0078] In the following examples, unless otherwise specified, all raw materials involved were commercially available analytically pure products.

[0079] Polyether polyol 2000: hydroxyl value of 54-58 mgKOH / g, acid value <0.5 mgKOH / g, purchased from Shandong Bluestar Dongda Co., Ltd.

[0080] Polyether polyol 3000: hydroxyl value is 36-39 mgKOH / g, acid value is <0.5 mgKOH / g, purchased from Shandong Bluestar Dongda Co., Ltd.

[0081] Polyester polyol: Polyester polyol 8651, 55-65 mgKOH / g, acid value ≤ 0.5 mgKOH / g, purchased from DIC Corporation.

[0082] Polyether EP-330NG: hydroxyl value is 32-36 mgKOH / g, acid value is ≤0.5 mgKOH / g, purchased from Shandong Bluestar Dongda Co., Ltd.

[0083] Curing agent BHD-8088 was purchased from Beijing Beihua Engineering Technology Co., Ltd.

[0084] The average particle size of the powder filler used below is 5 μm.

[0085] The total weight of the composition in each of the following examples is 2 kg, and the usage percentage of the components in each example is based on the total weight of the composition.

[0086] Preparation Example 1

[0087] This preparation example is used to prepare the first auxiliary agent used in Example 2, specifically comprising:

[0088] In the presence of cyclohexane, 2-methyl-1,5-pentanediamine and 30 g of benzaldehyde are contacted and mixed, and the product obtained after the contact and mixing is subjected to reduced pressure distillation to obtain the first auxiliary agent, which is named Z2;

[0089] The weight ratio of the benzaldehyde to the 2-methyl-1,5-pentanediamine is 1:0.39, and the amount of the cyclohexane is 3.3 mL for every 1 g of the benzaldehyde;

[0090] The contact mixing conditions include: temperature of 50°C and time of 6h;

[0091] The conditions of the reduced pressure distillation include: a temperature of 50° C. and a pressure of 0.2 MPa.

[0092] Example 1

[0093] This example is used to illustrate the preparation method of the polyurethane coating of the present invention. It includes:

[0094] (1) subjecting a polyether polyol to a first reaction with a plasticizer to obtain a material A;

[0095] (2) subjecting the material A to a second reaction with a powder filler, and further subjecting the product obtained after the second reaction to vacuum dehydration to obtain material B;

[0096] (3) subjecting the material B to a third reaction with diisocyanate to obtain material C;

[0097] (4) subjecting the material C to a fourth reaction with the first auxiliary agent, the second auxiliary agent and the solvent to obtain the polyurethane coating, wherein the fourth reaction is a vacuum degassing reaction;

[0098] The polyurethane coating prepared by the above method is named J-1.

[0099] Unless otherwise specified, the remaining examples were carried out using the same process as Example 1, but the formulations and process parameters used were different, as shown in Table 1.

[0100] Table 1

[0101]

[0102]

[0103] Comparative Example 1

[0104] This comparative example adopts a formula and method similar to that of Example 1 to prepare the coating, except that in this comparative example, the first auxiliary agent in Example 1 is replaced by an equal weight of curing agent BHD-8088. The polyurethane coating prepared by this method is named DJ-1.

[0105] Comparative Example 2

[0106] This comparative example adopts a formula and method similar to that of Example 1 to prepare the coating, except that in this comparative example, the polyether polyol in Example 1 is replaced by an equal weight of polyester polyol. The polyurethane coating prepared by this method is named DJ-2.

[0107] Comparative Example 3

[0108] This comparative example adopts a formula and method similar to that of Example 1 to prepare the coating, except that in this comparative example, the second auxiliary agent in Example 1 is replaced by an equal weight of stannous oleate. The polyurethane coating prepared by this method is named DJ-3.

[0109] Comparative Example 4

[0110] This comparative example adopts a formula and method similar to that of Example 1 to prepare the coating, except that in this comparative example, the amount of the first auxiliary agent is 6.5wt%, the amount of the diisocyanate is 1wt%, and the polyurethane coating prepared by this method is named DJ-4.

[0111] Comparative Example 5

[0112] This comparative example adopts a formula and method similar to that of Example 1 to prepare the coating, except that in this comparative example, the amount of the second auxiliary agent is 2wt%, the amount of the first auxiliary agent is 2wt%, and the polyurethane coating prepared by this method is named DJ-5.

[0113] Test Case

[0114] With reference to the standard GB / T 19250-2023 polyurethane waterproof coating, the performance of the polyurethane waterproof coating prepared above was tested. The specific results are shown in Table 2.

[0115] Table 2

[0116] Example 1 Example 2 Example 3 Example 4 Example 5 Polyurethane coating nomenclature J-1 J-2 J-3 J-4 J-5 Surface drying time (h) 4.5 4 5 5 5 Membrane status No bubbles No bubbles No bubbles No bubbles No bubbles Tensile strength(MPa) 4.0 4.1 3.9 3.5 3.4 Elongation at break (%) 550 525 558 567 560 Tear strength(N / mm) 28.3 33.6 31.5 26.6 27.3 Acid treatment tensile retention rate (%) 92 90 87 86 85 Alkali treatment tensile strength retention rate (%) 88 85 83 82 80 Heat treatment tensile strength retention rate (%) 89 86 87 84 85

[0117] Table 2

[0118] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Polyurethane coating nomenclature DJ-1 DJ-2 DJ-3 DJ-4 DJ-5 The first auxiliary type BHD-8088 Z3 Z2 Z1 Z1 Surface drying time (h) 6 5.5 5.5 6 6 Membrane status A few bubbles No bubbles No bubbles No bubbles No bubbles Tensile strength(MPa) 2.5 2.8 3.0 2.3 2.0 Elongation at break (%) 490 481 469 430 453 Tear strength (N / mm) 20.5 25.0 24.5 22.3 21.9 Acid treatment tensile retention rate (%) 72 79 80 76 73 Tensile strength retention after alkali treatment (%) 71 76 78 75 71 Heat treatment tensile strength retention rate (%) 72 79 76 73 70

[0119] It can be seen from the above results that the polyurethane waterproof coating prepared using the homemade latent curing agent has excellent properties such as surface drying time, film state, tensile strength, and elongation at break.

[0120] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A polyurethane coating composition, It is characterized in that The composition contains the following components which are stored separately: Diisocyanate, polyether polyol, powder filler, plasticizer, first auxiliary agent, second auxiliary agent and solvent; Based on the total weight of the coating, the content of the diisocyanate is 3-8wt%, the content of the polyether polyol is 20-40wt%, the content of the powder filler is 30-40wt%, the content of the plasticizer is 10-20wt%, the content of the first auxiliary agent is 2-6wt%, the content of the second auxiliary agent is 0.2-1.5wt%, and the content of the solvent is 4-15wt%; The polyether polyol has a hydroxyl value of 36-58 mgKOH / g and an acid value of ≤0.5 mgKOH / g; The first auxiliary agent is a structure shown in formula (I), The second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate; The first auxiliary agent is a product prepared by the following method, which comprises: In the presence of an organic solvent, 2-methyl-1,5-pentanediamine and benzaldehyde are contacted and mixed, and the product obtained after the contact and mixing is subjected to reduced pressure distillation to obtain an auxiliary material as the first auxiliary agent; The weight ratio of the benzaldehyde to the 2-methyl-1,5-pentanediamine is 1:0.2-0.40, and the amount of the organic solvent is 2-4 mL for every 1 g of the benzaldehyde; The contact mixing conditions include: temperature of 45-65°C and time of 5.5-6.5h; The conditions of the reduced pressure distillation treatment include: a temperature of 40-55° C. and a pressure of 0.1-0.5 MPa.

2. A composition according to claim 1, It is characterized in that The organic solvent is cyclohexane.

3. The composition according to claim 1 or 2, It is characterized in that The diisocyanate is selected from at least one of toluene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate; And / or, the polyether polyol is selected from at least one of polyether polyol 2000 and polyether polyol 3000.

4. Use of the composition described in any one of claims 1 to 3 in polyurethane coatings.

5. A method for preparing a polyurethane coating, It is characterized in that The method comprises: mixing and contacting the components in a composition containing diisocyanate, polyether polyol, powder filler, plasticizer, first auxiliary agent, second auxiliary agent and solvent to obtain the polyurethane coating; Based on the total amount of the composition, the amount of the diisocyanate is 3-8wt%, the amount of the polyether polyol is 20-40wt%, the amount of the powder filler is 30-40wt%, the amount of the plasticizer is 10-20wt%, the amount of the first auxiliary agent is 2-6wt%, the amount of the second auxiliary agent is 0.2-1.5wt%, and the amount of the solvent is 4-15wt%; The polyether polyol has a hydroxyl value of 36-58 mgKOH / g and an acid value of ≤0.5 mgKOH / g; The first auxiliary agent is a structure shown in formula (I), The second auxiliary agent is selected from at least one of dibutyltin dilaurate and stannous octoate; The first auxiliary agent is a product prepared by the following method, which comprises: In the presence of an organic solvent, 2-methyl-1,5-pentanediamine and benzaldehyde are contacted and mixed, and the product obtained after the contact and mixing is subjected to reduced pressure distillation to obtain an auxiliary material as the first auxiliary agent; The weight ratio of the benzaldehyde to the 2-methyl-1,5-pentanediamine is 1:0.2-0.40, and the amount of the organic solvent is 2-4 mL for every 1 g of the benzaldehyde; The contact mixing conditions include: temperature of 45-65°C and time of 5.5-6.5h; The conditions of the reduced pressure distillation treatment include: temperature of 40-55°C and pressure of 0.1-0.5MPa; The composition is the polyurethane coating composition according to any one of claims 1 to 3.

6. The method according to claim 5, It is characterized in that The steps of the mixed contact treatment include: (1) subjecting a polyether polyol to a first reaction with a plasticizer to obtain a material A; (2) subjecting the material A to a second reaction with a powder filler to obtain a material B; (3) subjecting the material B to a third reaction with diisocyanate to obtain material C; (4) subjecting the material C to a fourth reaction with the first auxiliary agent, the second auxiliary agent and the solvent to obtain the polyurethane coating.

7. The method according to claim 6, It is characterized in that In step (1), the conditions of the first reaction include: temperature of 70-90° C., stirring speed of 300-400 rpm, and stirring time of 0.3-0.8 h; And / or, in step (2), the conditions of the second reaction include: temperature of 100-120° C., stirring speed of 1100-1300 rpm, and stirring time of 0.3-0.8 h; And / or, in step (3), the conditions of the third reaction include: temperature of 40-60° C., stirring speed of 450-550 rpm, and stirring time of 1.5-2.5 h; And / or, in step (4), the conditions of the fourth reaction include: the vacuum degassing time is 40-50 min; the vacuum degassing pressure is -0.095 MPa to -0.1 MPa.

8. The method according to claim 6 or 7, It is characterized in that The method includes: (S1) preparing an auxiliary material as the first auxiliary agent: In the presence of an organic solvent, 2-methyl-1,5-pentanediamine and benzaldehyde are contacted and mixed, and the product obtained after the contact and mixing is subjected to reduced pressure distillation to obtain an auxiliary material as the first auxiliary agent; (S2) subjecting the polyether polyol and the plasticizer to the first reaction to obtain material A; (S3) subjecting the material A to the second reaction with the powder filler to obtain material B; (S4) subjecting the material B to the third reaction with diisocyanate to obtain material C; (S5) subjecting the material C to the fourth reaction with the auxiliary material, the second auxiliary agent and the solvent obtained in step (S1) to obtain the polyurethane coating.

9. The polyurethane coating prepared by the method described in any one of claims 6 to 8.

Citation Information

Patent Citations

  • Scraping-resistant water-based polyurethane paint

    CN107936647A

  • Modified single-component polyurethane waterproof coating composition, modified single-component polyurethane waterproof coating as well as preparation method and application of modified single-component polyurethane waterproof coating

    CN113444441A

  • Liquid aldimine latent curing agent as well as preparation method and application thereof

    CN117209702A