Anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls and preparation method thereof

By using composite fillers of titanium dioxide microspheres coated with ultraviolet absorption additives in acrylic resin coatings, the problem of insufficient heat insulation and anti-ultraviolet performance of existing coatings is solved, achieving better heat insulation and anti-ultraviolet effects, and improving the quality of buildings. Stability and durability of exterior paint.

CN117986951BActive Publication Date: 2024-09-27NANTONG LEJIA PAINT CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410170510.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2024-09-27
Estimated Expiration
2044-02-06

AI Technical Summary

Technical Problem

Existing acrylic resin coatings have insufficient performance in terms of heat insulation and UV resistance. In particular, the heat insulation performance needs to be improved, and UV absorption additives are easily degraded in high temperature environments, affecting the stability and durability of the material.

Method used

Titanium dioxide microspheres are used to coat ultraviolet absorption additive composite fillers. Hollow structure titanium dioxide microspheres are prepared through hydrothermal reaction and calcination steps, and ultraviolet absorption additives are coated on their surfaces to form composite fillers, combined with acrylic emulsion and other ingredients. Proceed with paint preparation.

Benefits of technology

Significantly improves the thermal insulation performance and UV resistance of the coating, enhances the stability and durability of the material, and provides better heat blocking and UV protection effects. It is suitable for building exterior walls that require both heat insulation and UV resistance. field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117986951B
    Figure CN117986951B
Patent Text Reader

Abstract

The invention relates to the field of building materials, and provides an anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls and a preparation method thereof. The coating comprises, by weight, 30 to 60 parts of titanium dioxide microspheres coated with ultraviolet absorption aid composite filler, 80 to 110 parts of acrylic emulsion, 40 to 90 parts of anhydrous ethanol, 5 to 12 parts of talcum powder, 1 to 6 parts of color enhancer, 2 to 5 parts of film former, 1 to 3 parts of dispersant, 1 to 3 parts of defoamer, 0.5 to 2 parts of leveling agent, 0.5 to 2 parts of preservative, and 1 to 3 parts of hydroxypropyl methylcellulose. First, titanium dioxide microspheres coated with ultraviolet absorption aid filler, anhydrous ethanol and hydroxypropyl methylcellulose, talcum powder and dispersant are stirred and mixed uniformly for standby use, and then acrylic emulsion, color enhancer, film former, defoamer, leveling agent, and preservative are added and stirred fully and uniformly. The coating of the invention has excellent heat insulation and anti-ultraviolet performance and has wide application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials, and in particular to an anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls and a preparation method thereof. Background Art

[0002] With climate change and increasing environmental awareness, the construction industry has higher and higher requirements for exterior wall coatings, especially in hot summers and cold winters, building exterior walls need to have good thermal insulation properties to reduce indoor temperature fluctuations and improve energy efficiency. In addition, damage to building exterior wall materials caused by ultraviolet radiation is also an important consideration. Long-term exposure to ultraviolet rays will cause fading of coating color and aging of the surface, reducing the aesthetics and durability of the building exterior wall. Therefore, finding a building exterior wall coating that can meet both thermal insulation and UV protection needs has become a hot topic in current research.

[0003] Acrylic resin is a polymer material with excellent physical and chemical properties, so it is widely used in many fields. First, acrylic resin has good weather resistance and durability, and can withstand the influence of external environment under various climatic conditions. Secondly, acrylic resin has good adhesion and wear resistance, which can effectively protect the substrate from external damage. In addition, acrylic resin also has good flexibility, making it an ideal coating material. Based on these characteristics, acrylic resin is widely used in the field of architectural coatings.

[0004] At present, the application of acrylic resin in building exterior wall coatings has made certain progress. By adding functional additives such as heat-insulating fillers and ultraviolet absorbers to acrylic resin, the heat-insulating performance and ultraviolet resistance of the coating can be significantly improved. However, the current acrylic resin coatings still have some shortcomings in terms of heat insulation and ultraviolet protection. 1. The heat-insulating performance needs to be improved. For example, the Chinese patent with publication number CN111499816A discloses a nano-SiO2 modified acrylic resin. The research results show that the modified acrylic resin has a good ultraviolet shielding effect, but nano-SiO2 is a solid filler and still has a certain thermal conductivity. Therefore, the heat-insulating performance of the modified acrylic ester needs to be improved. 2. The thermal stability of the ultraviolet absorption additive needs to be improved. Ultraviolet absorption additives are usually directly added in the traditional coating preparation process. For example, the Chinese patent with publication number CN108047853A discloses a coating containing ultraviolet absorption additives, but in actual application, ultraviolet radiation under high temperature environment will cause the additive to degrade, volatilize or fail, thereby weakening the material's protection effect against ultraviolet rays. This not only affects the performance stability of the material, but may also cause fading, aging, cracking and other damage to the material. Therefore, acrylic resin coatings currently still face many challenges in terms of heat insulation and UV resistance. In order to fill this technical gap, it is necessary to develop a new type of acrylic resin coating that has both heat insulation and excellent UV resistance to meet the demand for high-performance acrylic resin coatings for building exterior walls.

[0005] The invention provides an anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls and a preparation method thereof, so as to solve the problem that the current acrylic resin has insufficient heat-insulating performance and anti-ultraviolet performance. Summary of the invention

[0006] (1) Technical issues solved

[0007] The purpose of the present invention is to provide an anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls and a preparation method thereof, so as to solve the problem that the current acrylic resin has insufficient heat-insulating performance and anti-ultraviolet performance.

[0008] (2) Technical solution

[0009] In order to achieve the above object, the present invention provides the following technical solutions:

[0010] An anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls comprises the following components by weight: 30-60 parts of titanium dioxide microspheres coated with ultraviolet absorption aid composite filler, 80-110 parts of acrylic emulsion, 40-90 parts of anhydrous ethanol, 5-12 parts of talcum powder, 1-6 parts of color enhancer, 2-5 parts of film former, 1-3 parts of dispersant, 1-3 parts of defoamer, 0.5-2 parts of leveling agent, 0.5-2 parts of preservative, and 1-3 parts of hydroxypropyl methylcellulose. The average size of the titanium dioxide microspheres coated with ultraviolet absorption aid composite filler is 50-200nm.

[0011] Furthermore, the preparation method of the titanium dioxide microspheres is as follows: 10 to 20 parts of fructose and 2 to 6 parts of sodium dodecyl sulfate are placed in 20 to 40 parts of a mixed solution of water and anhydrous ethanol in a volume ratio of 1:1, stirred evenly, placed in a high-pressure reactor, hydrothermally reacted at 160 to 250° C. for 12 to 24 hours, cooled, washed, filtered, and vacuum dried to obtain carbon hollow microspheres; then 20 to 40 parts of carbon hollow microspheres, 5 to 10 titanium salts and 2 to 6 parts of hexadecyl polyoxyethylene ether are dissolved in 100 parts of anhydrous ethanol, stirred evenly, placed in a high-pressure reactor, hydrothermally reacted at 120 to 160° C. for 6-12 hours, and then naturally cooled, filtered, washed and dried to obtain titanium-containing compound-coated carbon hollow microspheres; finally, calcined at 500 to 600° C. for 2 to 4 hours in an air atmosphere to finally obtain hollow structure titanium dioxide microspheres.

[0012] Furthermore, the titanium salt is a mixture of one or more of sodium titanate and potassium titanate.

[0013] Furthermore, the ultraviolet absorption aid is 2-chloro-4-nitrophenyloxyethyl methylcyclohexane.

[0014] Furthermore, the preparation method of the titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent filler is as follows: in parts by weight, first, 10 to 20 parts of nitrophenol and 30 to 60 parts of 2-bromoethanol are mixed evenly in 50 to 100 parts of dichloromethane solvent, and reacted at 50 to 80° C. for 2 to 4 hours to generate an aromatic ether compound; then, 10 to 40 parts of 2-chloroethanol are added and stirred thoroughly, and then 30 to 60 parts of titanium dioxide microspheres are added, and the mixture is reacted at 80 to 120° C. for 4 to 12 hours to generate 2-chloro-4-nitrophenyloxyethylmethylcyclohexane in the hollow titanium dioxide microspheres; finally, the titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent composite filler is obtained after washing and vacuum drying.

[0015] Furthermore, the mass ratio of the nitrophenol, 2-bromoethanol and 2-chloroethanol is 1:3:(1-2).

[0016] Furthermore, the preparation method of the acrylic emulsion is as follows: by weight, 4 to 10 parts of acrylic acid, 5 to 10 parts of ethyl acrylate, 30 to 50 parts of anhydrous ethanol and 3 to 6 parts of sodium dodecylbenzene sulfonate are stirred uniformly to form a mixed solution, and then 2 to 4 parts of ammonium persulfate are added to form an acrylic emulsion.

[0017] Furthermore, the film-forming agent is a mixture of one or more of lauryl alcohol ester and polyethyl acrylate.

[0018] Furthermore, the dispersant is a mixture of one or more of cetyltrimethylammonium bromide and polyethylene glycol.

[0019] Furthermore, the defoaming agent is a mixture of one or more of polydimethylsiloxane, oleate, and fatty alcohol polyoxyethylene ether.

[0020] Furthermore, the leveling agent is a mixture of one or more of polydimethylsiloxane and trimethylolaminomethane.

[0021] Furthermore, the preservative is any one of benzoic acid and sodium copper ethylenediaminetetraacetate.

[0022] The present invention also provides a method for preparing an anti-ultraviolet acrylic resin heat-insulating coating for a building exterior wall, comprising:

[0023] S1. Prepare acrylic emulsion: stir acrylic acid, ethyl acrylate, anhydrous ethanol and sodium dodecylbenzene sulfonate to form a mixed solution, and then add ammonium persulfate to form an acrylic emulsion for use.

[0024] S2. Preparation of titanium dioxide microspheres coated with ultraviolet absorption additive filler: fructose and sodium dodecyl sulfate are dissolved in a mixed solution of water and anhydrous ethanol, and then carbon hollow microspheres are prepared by hydrothermal reaction at high temperature. Next, the carbon hollow microspheres are mixed with titanium salt and hexadecyl polyoxyethylene ether in anhydrous ethanol, and then hydrothermally reacted and calcined to obtain titanium dioxide microspheres. Finally, nitrophenol is reacted with 2-bromoethanol to generate an aromatic ether compound, which is then reacted with 2-chloroethanol and titanium dioxide microspheres to generate titanium dioxide microspheres coated with ultraviolet absorption additive filler.

[0025] S3. Dispersing solid fillers: According to the proportions, titanium dioxide microspheres coated with ultraviolet light absorbing additive fillers, anhydrous ethanol and hydroxypropyl methylcellulose, talcum powder and dispersants are mixed evenly in a mixer to obtain evenly dispersed solid fillers for use.

[0026] S4. Prepare the coating: add acrylic emulsion, evenly dispersed solid filler, titanium dioxide microsphere-coated ultraviolet absorption additive filler, color enhancer, film former, defoamer, leveling agent, and preservative into a high-speed mixer and stir thoroughly.

[0027] The present invention realizes the construction of a composite structure containing carbon hollow microspheres and titanium compounds by introducing multi-component materials such as fructose, sodium dodecyl sulfate and titanium salts during the preparation of titanium dioxide microspheres. Secondly, by using a hydrothermal reaction method, the reaction is carried out at a relatively high temperature and pressure, which promotes the uniform mixing of materials and the full progress of the reaction, and is conducive to improving the crystallinity and grain size of the materials, thereby improving the reaction efficiency. In addition, by coating the surface of the carbon hollow microspheres with titanium-containing compounds, a uniform structural layer is formed. The final calcination step further improves the crystal structure and stability of the material, and realizes the preparation of titanium dioxide microspheres with a hollow structure. The preparation method realizes the preparation of titanium dioxide microspheres with a hollow structure through the construction of multi-component materials, the use of hydrothermal reactions, the introduction of coating layers and the treatment of calcination, and has good structural stability.

[0028] (3) Beneficial technical effects

[0029] The anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls of the present invention achieves multiple beneficial effects:

[0030] 1. Titanium dioxide microspheres have excellent thermal insulation properties. The microsphere structure has a large surface area and can form a barrier layer for heat conduction, effectively reducing heat transfer. Compared with solid titanium dioxide microspheres, it has better thermal insulation effect.

[0031] 2. When ultraviolet rays irradiate the surface of the material, titanium dioxide microspheres can absorb ultraviolet energy and convert it into heat. This heat absorption and conduction process can further increase the thermal insulation effect of the material, reduce the transmission of heat to the inside, and help improve the thermal stability of the internal ultraviolet absorption additive at high temperatures, and improve the stability and long-term effectiveness of the ultraviolet absorption additive.

[0032] 3. The UV absorbing additives encapsulated in the titanium dioxide microspheres have excellent UV absorption capabilities. These absorbing additives can further absorb UV rays, reduce the damage of UV rays to materials, and convert their energy into heat or other forms of energy.

[0033] 4. The titanium dioxide microspheres are coated with ultraviolet absorption additives, which have better heat insulation effect than traditional solid titanium dioxide microspheres.

[0034] 5. Titanium dioxide microspheres can also be used as a protective shell for ultraviolet absorption aids to protect and stabilize ultraviolet absorption aids, prevent the absorbent from dissolving or decomposing, and further enhance the stability of the material. The two work together to enhance the thermal insulation effect of the material and improve the material's ability to protect against ultraviolet rays. This synergistic effect can greatly improve the performance and stability of the material, and is widely used in the field of building materials that require both thermal insulation and anti-ultraviolet functions.

[0035] In summary, titanium dioxide microspheres coated with ultraviolet absorbing additive fillers overcome the problem that adding thermal insulation fillers and ultraviolet absorbing additives separately in traditional coatings cannot further improve the thermal insulation effect and UV resistance. It can achieve the synergistic improvement of acrylic resin thermal insulation and UV resistance, improve the performance and stability of coatings for building exterior walls, and has broad application prospects in fields such as building materials that require both thermal insulation and UV resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a low-magnification morphology image of the hollow titanium dioxide microspheres prepared in Example 1 of the present invention.

[0037] Figure 2 This is a high-magnification morphology image of the hollow titanium dioxide microspheres encapsulating the ultraviolet absorbing agent prepared in Example 1 of the present invention.

[0038] Figure 3 This is the XRD phase analysis diagram of the hollow titanium dioxide microspheres prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0039] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0040] In the case of not specifying specific conditions, the operation in the examples is carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not indicated, are all common products on the market. Parts not mentioned in the technical content of the present invention will be processed with reference to the prior art. Unless otherwise specified, the following examples and comparative examples will be tested in parallel and use the same processing steps and parameters.

[0041] Table 1 below shows the reagents required for the examples and the corresponding purchasing companies.

[0042] Table 1 Reagents required for the examples and corresponding purchasing companies

[0043]

[0044]

[0045] Example 1

[0046] An anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls comprises the following components by weight: 30 parts of titanium dioxide microspheres coated with ultraviolet absorption aid composite filler, 80 parts of acrylic emulsion, 40 parts of anhydrous ethanol, 5 parts of talcum powder, 1 part of color enhancer, 2 parts of film former, 1 part of dispersant, 1 part of defoamer, 0.5 parts of leveling agent, 0.5 parts of preservative, and 1 part of hydroxypropyl methylcellulose. The average size of the titanium dioxide microspheres coated with ultraviolet absorption aid composite filler is 55nm.

[0047] The preparation method of the above-mentioned titanium dioxide microspheres is as follows: 10 parts of fructose and 2 parts of sodium dodecyl sulfate are placed in 20 parts of a mixed solution of water and anhydrous ethanol in a volume ratio of 1:1, stirred evenly and placed in a high-pressure reactor, hydrothermally reacted at 160°C for 12 hours, cooled and washed, filtered, and vacuum dried to obtain carbon hollow microspheres; then 20 parts of carbon hollow microspheres, 5 parts of salt and 2 parts of hexadecyl polyoxyethylene ether are dissolved in 100 parts of anhydrous ethanol, stirred evenly and placed in a high-pressure reactor, hydrothermally reacted at 120°C for 6 hours, and then naturally cooled, filtered, washed and dried to obtain titanium-containing compound-coated carbon hollow microspheres; finally, calcined at 500°C for 2 hours in an air atmosphere to finally obtain hollow titanium dioxide microspheres.

[0048] The titanium salt is sodium titanate.

[0049] The ultraviolet absorption aid is 2-chloro-4-nitrophenyloxyethylmethylcyclohexane.

[0050] The preparation method of the above-mentioned titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent filler is as follows: in parts by weight, first, 10 parts of nitrophenol and 30 parts of 2-bromoethanol are mixed evenly in 50 parts of dichloromethane solvent, and reacted at 50°C for 2 hours to generate an aromatic ether compound; then 20 parts of 2-chloroethanol are added and stirred thoroughly, and then 30 parts of titanium dioxide microspheres are added, and the mixture is reacted at 80°C for 4 hours to generate 2-chloro-4-nitrophenyloxyethylmethylcyclohexane in the hollow titanium dioxide microspheres; finally, the titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent composite filler is obtained after washing and vacuum drying.

[0051] The mass ratio of the above-mentioned nitrophenol, 2-bromoethanol and 2-chloroethanol is 1:3:2.

[0052] The preparation method of the acrylic emulsion is as follows: by weight, 4 parts of acrylic acid, 5 parts of ethyl acrylate, 30 parts of anhydrous ethanol and 3 parts of sodium dodecylbenzene sulfonate are stirred uniformly to form a mixed solution, and then 2 parts of ammonium persulfate are added to form an acrylic emulsion.

[0053] The above-mentioned film former is dodecyl alcohol ester.

[0054] The above dispersant is hexadecyltrimethylammonium bromide.

[0055] The defoaming agent is polydimethylsiloxane.

[0056] The above-mentioned leveling agent is polydimethylsiloxane.

[0057] The above-mentioned preservative is benzoic acid.

[0058] The present invention also provides a method for preparing an anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls:

[0059] S1. Prepare acrylic emulsion: stir acrylic acid, ethyl acrylate, anhydrous ethanol and sodium dodecylbenzene sulfonate to form a mixed solution, and then add ammonium persulfate to form an acrylic emulsion for use.

[0060] S2. Preparation of titanium dioxide microspheres coated with ultraviolet absorption additive filler: fructose and sodium dodecyl sulfate are dissolved in a mixed solution of water and anhydrous ethanol, and then carbon hollow microspheres are prepared by hydrothermal reaction at high temperature. Next, the carbon hollow microspheres are mixed with titanium salt and hexadecyl polyoxyethylene ether in anhydrous ethanol, and then hydrothermally reacted and calcined to obtain titanium dioxide microspheres. Finally, nitrophenol is reacted with 2-bromoethanol to generate an aromatic ether compound, which is then reacted with 2-chloroethanol and titanium dioxide microspheres to generate titanium dioxide microspheres coated with ultraviolet absorption additive filler.

[0061] S3. Dispersing solid fillers: According to the proportions, titanium dioxide microspheres coated with ultraviolet light absorbing additive fillers, anhydrous ethanol and hydroxypropyl methylcellulose, talcum powder and dispersants are mixed evenly in a mixer to obtain evenly dispersed solid fillers for use.

[0062] S4. Prepare the coating: add acrylic emulsion, evenly dispersed solid filler, titanium dioxide microsphere-coated ultraviolet absorption additive filler, color enhancer, film-forming agent, defoamer, leveling agent, and preservative into a high-speed mixer and stir thoroughly.

[0063] Example 2

[0064] An anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls comprises the following components by weight: 40 parts of titanium dioxide microspheres coated with ultraviolet absorption aid composite filler, 90 parts of acrylic emulsion, 50 parts of anhydrous ethanol, 6 parts of talcum powder, 2 parts of color enhancer, 3 parts of film former, 1.5 parts of dispersant, 1.5 parts of defoamer, 1 part of leveling agent, 1 part of preservative, and 1.5 parts of hydroxypropyl methylcellulose. The average size of the titanium dioxide microspheres coated with ultraviolet absorption aid composite filler is 80nm.

[0065] The preparation method of the above-mentioned titanium dioxide microspheres is as follows: 10 to 20 parts of fructose and 2 to 6 parts of sodium dodecyl sulfate are placed in 20 to 40 parts of a mixed solution of water and anhydrous ethanol in a volume ratio of 1:1, stirred evenly, placed in a high-pressure reactor, hydrothermally reacted at 160 to 250°C for 12 to 24 hours, cooled, washed, filtered, and vacuum dried to obtain carbon hollow microspheres; then 20 to 40 parts of carbon hollow microspheres, 5 to 10 titanium salts and 2 to 6 parts of hexadecyl polyoxyethylene ether are dissolved in 100 parts of anhydrous ethanol, stirred evenly, placed in a high-pressure reactor, hydrothermally reacted at 120 to 160°C for 6-12 hours, and then naturally cooled, filtered, washed and dried to obtain titanium-containing compound-coated carbon hollow microspheres; finally, calcined at 500 to 600°C for 2 to 4 hours in an air atmosphere to finally obtain hollow structure titanium dioxide microspheres.

[0066] The above-mentioned titanium salt is potassium titanate.

[0067] The ultraviolet absorption aid is 2-chloro-4-nitrophenyloxyethylmethylcyclohexane.

[0068] The preparation method of the above-mentioned titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent filler is as follows: in parts by weight, first, 12 parts of nitrophenol and 36 parts of 2-bromoethanol are mixed evenly in 60 parts of dichloromethane solvent, and reacted at 60°C for 2.5 hours to generate an aromatic ether compound; then 12 parts of 2-chloroethanol are added and stirred thoroughly, and then 40 parts of titanium dioxide microspheres are added, and the mixture is reacted at 90°C for 6 hours to generate 2-chloro-4-nitrophenyloxyethylmethylcyclohexane in the hollow titanium dioxide microspheres; finally, the titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent composite filler is obtained after washing and vacuum drying.

[0069] The mass ratio of the above-mentioned nitrophenol, 2-bromoethanol and 2-chloroethanol is 1:3:1.

[0070] The preparation method of the acrylic emulsion is as follows: by weight, 6 parts of acrylic acid, 6 parts of ethyl acrylate, 40 parts of anhydrous ethanol and 4 parts of sodium dodecylbenzene sulfonate are stirred uniformly to form a mixed solution, and then 2 to 4 parts of ammonium persulfate are added to form an acrylic emulsion.

[0071] The above film-forming agent is polyethyl acrylate.

[0072] The above dispersant is polyethylene glycol.

[0073] The above defoaming agent is oleic acid ester.

[0074] The leveling agent is tris(hydroxymethyl)aminomethane.

[0075] The preservative is sodium copper ethylenediaminetetraacetate.

[0076] The present invention also provides a method for preparing an anti-ultraviolet acrylic resin thermal insulation coating for building exterior walls, which is the same as that in Example 1 and will not be described in detail herein.

[0077] Example 3

[0078] An anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls comprises the following components by weight: 50 parts of titanium dioxide microspheres coated with ultraviolet absorption aid composite filler, 100 parts of acrylic emulsion, 80 parts of anhydrous ethanol, 10 parts of talcum powder, 3 parts of color enhancer, 4 parts of film former, 2 parts of dispersant, 2 parts of defoamer, 1 part of leveling agent, 1 part of preservative, and 2 parts of hydroxypropyl methylcellulose. The average size of the titanium dioxide microspheres coated with ultraviolet absorption aid composite filler is 120nm.

[0079] The preparation method of the above-mentioned titanium dioxide microspheres is as follows: 15 parts of fructose and 4 parts of sodium dodecyl sulfate are placed in 35 parts of a mixed solution of water and anhydrous ethanol with a volume ratio of 1:1, stirred evenly and placed in a high-pressure reactor, hydrothermally reacted at 200°C for 20 hours, cooled and washed, filtered, and vacuum dried to obtain carbon hollow microspheres; then 35 parts of carbon hollow microspheres, 7 parts of salt and 5 parts of hexadecyl polyoxyethylene ether are dissolved in 100 parts of anhydrous ethanol, stirred evenly and placed in a high-pressure reactor, hydrothermally reacted at 140°C for 10 hours, and then naturally cooled, filtered, washed and dried to obtain titanium-containing compound-coated carbon hollow microspheres; finally, calcined at 550°C for 3.5 hours in an air atmosphere to finally obtain hollow titanium dioxide microspheres.

[0080] The titanium salt is a mixture of sodium titanate and potassium titanate in a mass ratio of 1:2.

[0081] The ultraviolet absorption aid is 2-chloro-4-nitrophenyloxyethylmethylcyclohexane.

[0082] The preparation method of the above-mentioned titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent filler is as follows: in parts by weight, first, 16 parts of nitrophenol and 48 parts of 2-bromoethanol are mixed evenly in 80 parts of dichloromethane solvent, and reacted at 70°C for 3 hours to generate an aromatic ether compound; then 32 parts of 2-chloroethanol are added and stirred thoroughly, and then 50 parts of titanium dioxide microspheres are added, and the mixture is reacted at 100°C for 10 hours to generate 2-chloro-4-nitrophenyloxyethylmethylcyclohexane in the hollow titanium dioxide microspheres; finally, the titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent composite filler is obtained after washing and vacuum drying.

[0083] The mass ratio of the above-mentioned nitrophenol, 2-bromoethanol and 2-chloroethanol is 1:3:2.

[0084] The preparation method of the acrylic emulsion is as follows: by weight, 8 parts of acrylic acid, 8 parts of ethyl acrylate, 40 parts of anhydrous ethanol and 5 parts of sodium dodecylbenzene sulfonate are stirred uniformly to form a mixed solution, and then 3 parts of ammonium persulfate are added to form an acrylic emulsion.

[0085] The above film-forming agent is polyethyl acrylate.

[0086] The above dispersant is cetyltrimethylammonium bromide and polyethylene glycol mixed in a mass ratio of 1:1.

[0087] The above defoaming agent is fatty alcohol polyoxyethylene ether.

[0088] The above-mentioned leveling agent is polydimethylsiloxane.

[0089] The preservative is sodium copper ethylenediaminetetraacetate.

[0090] The present invention also provides a method for preparing an anti-ultraviolet acrylic resin thermal insulation coating for building exterior walls, which is the same as that in Example 1 and will not be described in detail herein.

[0091] Example 4

[0092] An anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls comprises the following components by weight: 60 parts of titanium dioxide microspheres coated with ultraviolet absorption aid composite filler, 110 parts of acrylic emulsion, 90 parts of anhydrous ethanol, 12 parts of talcum powder, 6 parts of color enhancer, 5 parts of film former, 3 parts of dispersant, 3 parts of defoamer, 2 parts of leveling agent, 2 parts of preservative, and 3 parts of hydroxypropyl methylcellulose. The average size of the titanium dioxide microspheres coated with ultraviolet absorption aid composite filler is 200nm.

[0093] The preparation method of the above-mentioned titanium dioxide microspheres is as follows: 20 parts of fructose and 6 parts of sodium dodecyl sulfate are placed in 40 parts of a mixed solution of water and anhydrous ethanol in a volume ratio of 1:1, stirred evenly and placed in a high-pressure reactor, hydrothermally reacted at 250°C for 24 hours, cooled and washed, filtered, and vacuum dried to obtain carbon hollow microspheres; then 40 parts of carbon hollow microspheres, 10 titanium salts and 6 parts of hexadecyl polyoxyethylene ether are dissolved in 100 parts of anhydrous ethanol, stirred evenly and placed in a high-pressure reactor, hydrothermally reacted at 160°C for 12 hours, and then naturally cooled, filtered, washed and dried to obtain titanium-containing compound-coated carbon hollow microspheres; finally, calcined at 600°C for 4 hours in an air atmosphere to finally obtain hollow titanium dioxide microspheres.

[0094] The titanium salt is a mixture of one or more of sodium titanate and potassium titanate.

[0095] The ultraviolet absorption aid is 2-chloro-4-nitrophenyloxyethylmethylcyclohexane.

[0096] The preparation method of the above-mentioned titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent filler is as follows: in parts by weight, first, 20 parts of nitrophenol and 60 parts of 2-bromoethanol are mixed evenly in 100 parts of dichloromethane solvent, and reacted at 80°C for 4 hours to generate an aromatic ether compound; then 40 parts of 2-chloroethanol are added and stirred thoroughly, and then 60 parts of titanium dioxide microspheres are added, and the mixture is reacted at 120°C for 12 hours to generate 2-chloro-4-nitrophenyloxyethylmethylcyclohexane in the hollow titanium dioxide microspheres; finally, the titanium dioxide microsphere-coated ultraviolet absorption auxiliary agent composite filler is obtained after washing and vacuum drying.

[0097] The mass ratio of the above-mentioned nitrophenol, 2-bromoethanol and 2-chloroethanol is 1:3:2.

[0098] The preparation method of the acrylic emulsion is as follows: by weight, 10 parts of acrylic acid, 10 parts of ethyl acrylate, 50 parts of anhydrous ethanol and 6 parts of sodium dodecylbenzene sulfonate are stirred uniformly to form a mixed solution, and then 4 parts of ammonium persulfate are added to form an acrylic emulsion.

[0099] The above film-forming agent is polyethyl acrylate.

[0100] The above dispersant is polyethylene glycol.

[0101] The above defoaming agent is oleic acid ester.

[0102] The leveling agent is tris(hydroxymethyl)aminomethane.

[0103] The preservative is sodium copper ethylenediaminetetraacetate.

[0104] The present invention also provides a method for preparing an anti-ultraviolet acrylic resin thermal insulation coating for building exterior walls, which is the same as that in Example 1 and will not be described in detail herein.

[0105] Example 5

[0106] It is basically the same as Example 1, except that the amount of the titanium dioxide microsphere-coated ultraviolet absorption aid composite filler is 50 parts.

[0107] Example 6

[0108] It is basically the same as Example 1, except that the average size of the titanium dioxide microspheres encapsulating the ultraviolet absorbing additive composite filler is 100 nm.

[0109] Comparative Example 1

[0110] The method is basically the same as Example 1, except that the coating does not contain titanium dioxide microspheres or a composite filler coated with an ultraviolet light absorbing agent.

[0111] Comparative Example 2

[0112] The method is basically the same as Example 1, except that the titanium dioxide microspheres are not coated with the ultraviolet absorbing agent, but hollow titanium dioxide microspheres are directly used.

[0113] Comparative Example 3

[0114] It is basically the same as Example 1, except that the ultraviolet absorbing agent is not coated with titanium dioxide microspheres, but is directly used as the ultraviolet absorbing agent.

[0115] Comparative Example 4

[0116] It is basically the same as Example 1, except that titanium dioxide is not used to coat the ultraviolet absorbing agent. Instead, an equal mass of titanium dioxide hollow microspheres and a mixture of ultraviolet absorbing agents are added separately when preparing the coating. Therefore, the titanium dioxide microspheres and the ultraviolet absorbing agents in Example 4 do not form a coating structure.

[0117] Comparative Example 5

[0118] It is basically the same as Example 1, except that the composite filler is solid titanium dioxide microspheres, and therefore is not coated with an ultraviolet absorbing agent.

[0119] Characterization Tests:

[0120] The present invention uses a scanning electron microscope to observe the morphology of the titanium dioxide microspheres prepared in Example 1, and it can be seen that the prepared titanium dioxide microspheres are uniform in size and well dispersed, which makes them perform well in heat insulation and UV resistance. The uniform size distribution can ensure that the microspheres can be evenly distributed inside the coating during the coating or wrapping process, thereby providing better heat insulation and UV resistance.

[0121] from Figure 2 for Figure 1 In the microscopic photo of titanium dioxide microspheres coated with UV absorbing agents, it can be seen that the hollow microsphere structure is obvious, which provides a good structural basis for its encapsulation of anti-UV additives. The coated UV absorbing agents can be clearly seen inside the microsphere structure. In addition, such a coating structure increases the contact area between titanium dioxide microspheres and UV absorbing agents, further improving the anti-UV performance.

[0122] Figure 3 The results of the phase analysis of the titanium dioxide microspheres prepared in Example 1 show that the titanium dioxide microspheres prepared in Example 1 contain only titanium dioxide phase, which means that no impurities or other undesirable substances are present in the preparation process. Pure titanium dioxide microspheres can better exert their heat insulation and UV resistance properties, ensuring their high efficiency and long-term stability.

[0123] Performance Testing:

[0124] Thermal insulation performance is one of the important indicators of coatings in building exterior wall applications. The thermal insulation performance test of coatings refers to GB / T 23987-2009 "Architectural coatings and their raw materials - thermal insulation coatings", which mainly evaluates thermal insulation performance by the size of thermal conductivity. The lower the thermal conductivity, the better the thermal insulation. The test can evaluate the thermal insulation performance of acrylic resin coatings, thus providing a basis for its application in the field of coating thermal insulation.

[0125] UV resistance is also one of the important properties that need to be considered for building exterior wall coatings. The UV resistance test is tested according to the ASTM D4587 standard. This method requires that the coating samples be exposed to natural sunlight and the UV resistance of the coating be evaluated by regularly evaluating its surface changes, color changes, adhesion, strength loss and other indicators. The test results of the coating are divided into five levels according to the degree of change, from best to worst, namely 0, 1, 2, 3 and 4. Among them, 0 represents no change, 1 and 2 represent slight changes, 3 represents moderate changes, and 4 represents severe changes.

[0126] The thermal conductivity and UV resistance levels of the coatings of Examples 1 to 6 and Comparative Examples 1 to 5 are summarized in Table 2.

[0127] Table 2 Thermal conductivity and UV resistance of coatings of Examples 1 to 6 and Comparative Examples 1 to 5

[0128]

[0129] The main difference between Example 1 and Comparative Example 1 is whether titanium dioxide microspheres are coated with ultraviolet absorption aid composite fillers. This difference leads to significant differences in thermal conductivity and ultraviolet protection levels between the two. In terms of thermal conductivity, since titanium dioxide microspheres are used in Example 1, its thermal conductivity is relatively low, which is 0.028W / (m·K), showing good thermal insulation performance. However, Comparative Example 1 does not use titanium dioxide microspheres, and its thermal conductivity is relatively high, which is 0.08W / (m·K). In terms of ultraviolet protection level, since the titanium dioxide microspheres in Example 1 are coated with ultraviolet absorption aids, its ultraviolet protection level is 0, showing good anti-ultraviolet performance. However, Comparative Example 1 does not add titanium dioxide microspheres and ultraviolet absorption aids, and its ultraviolet protection level is relatively low, only level 2. In terms of ultraviolet protection level after 100 days, since the titanium dioxide microspheres in Example 1 have a stable coating structure, its ultraviolet protection level is still 0, showing long-lasting anti-ultraviolet protection. The ultraviolet protection level of Comparative Example 1 is reduced to level 4 under long-term exposure.

[0130] There is a significant difference between Comparative Example 2 and Example 1 in terms of material composition, namely, whether the titanium dioxide microspheres are coated with ultraviolet absorption aids. By comparing the thermal conductivity and ultraviolet protection level of the two, and conducting in-depth analysis in combination with relevant mechanisms, we draw the following conclusions: Comparative Example 2 uses titanium dioxide microspheres with a hollow structure, which reduces its thermal conductivity to 0.016W / (m·K), which is lower than 0.028W / (m·K) of Example 1. However, since Comparative Example 2 is not coated with ultraviolet absorption aids, its anti-ultraviolet performance is poor, and the ultraviolet protection level is only level 1, while Example 1 reaches level 0. In addition, after long-term exposure (100 days), the ultraviolet protection level of Comparative Example 2 is increased to level 2, while Example 1 remains unchanged. Therefore, when choosing a coating, we should comprehensively consider thermal conductivity and ultraviolet resistance. The combination of titanium dioxide microspheres and ultraviolet absorption aids used in Example 1 is a more ideal choice.

[0131] A significant difference between Comparative Example 3 and Example 1 is whether titanium dioxide microspheres are used to coat the ultraviolet absorbing agent. By comparing the thermal conductivity and UV protection level of the two, and combining the relevant mechanism analysis, we draw the following conclusions: Since the titanium dioxide microspheres in Example 1 have a coating structure, their thermal conductivity is relatively low, only 0.028W / (m·K), and it also provides a certain degree of anti-ultraviolet protection for the material. In contrast, Comparative Example 3 directly uses ultraviolet absorbing agents, resulting in a higher thermal conductivity of 0.07W / (m·K). Due to the lack of thermal insulation effect of titanium dioxide microspheres, the UV protection level of Comparative Example 3 is also low.

[0132] In Comparative Example 4, the titanium dioxide microspheres and the ultraviolet absorption aid did not form a coating structure. By comparing the thermal conductivity and ultraviolet protection level of Example 1 and Comparative Example 4, and conducting in-depth analysis in combination with the relevant mechanisms, we have drawn several important conclusions. First, in terms of thermal conductivity, Example 1 exhibits a lower thermal conductivity of 0.028W / (m·K). In contrast, the thermal conductivity of Comparative Example 4 is slightly higher, reaching 0.032W / (m·K). This difference is mainly attributed to the separate addition of titanium dioxide microspheres and ultraviolet absorption aids in Comparative Example 4. The heat insulation effect of the filler in this way is worse than that of the coated filler, resulting in a slight increase in the thermal conductivity of the material. Secondly, in terms of ultraviolet protection performance, Example 1 performs well, and its ultraviolet protection level is maintained at level 0. After 100 days of exposure testing, the ultraviolet protection level of Example 1 remains stable at level 0. However, it is worth noting that the ultraviolet protection level of Comparative Example 4 has improved after the same exposure period, reaching level 3. This result shows that titanium dioxide can effectively improve the stability of anti-UV absorbing additives, and titanium dioxide hollow microspheres play an important role in enhancing anti-UV stability, thereby improving the overall anti-UV ability of the material.

[0133] The main difference between Comparative Example 5 and Example 1 is whether the titanium dioxide microspheres are solid or coated with ultraviolet absorbing agents. In terms of thermal conductivity, the thermal conductivity of Example 1 is 0.028W / (m·K), while the thermal conductivity of Comparative Example 5 is slightly higher, at 0.034W / (m·K). This may be due to the fact that Comparative Example 5 uses solid titanium dioxide microspheres, whose thermal conductivity is slightly higher than that of ordinary titanium dioxide microspheres, resulting in an increase in the thermal conductivity of the overall material. In terms of UV protection level, Example 1 exhibits excellent UV resistance, with a UV protection level of 0. However, the UV protection level of Comparative Example 5 is only level 1, which may be because the UV resistance of its core titanium dioxide microspheres is relatively weak. After 100 days of exposure, the UV protection level of Example 1 is still level 0, while the UV protection level of Comparative Example 5 has been increased to level 2. This may be because the titanium dioxide microspheres in Example 1 are coated with anti-ultraviolet absorbing agents, which can provide long-lasting anti-ultraviolet protection, further improving the UV protection level.

[0134] In summary, the titanium dioxide microspheres coated with anti-ultraviolet absorbing aids in the present invention show a significant synergistic effect. It not only provides excellent anti-ultraviolet protection, but also exhibits excellent thermal insulation performance. By uniformly coating the anti-ultraviolet absorbing aid on the surface of the titanium dioxide microspheres, we have successfully enhanced the anti-ultraviolet ability of the material, enabling it to more effectively absorb, reflect or scatter ultraviolet rays, significantly reducing the damage of ultraviolet rays to objects. At the same time, the titanium dioxide microspheres themselves have a low thermal conductivity, which can effectively reduce the conduction of heat, block the loss of heat and the entry of external heat, and provide excellent thermal insulation effect. This unique coating structure also ensures good durability and durability, so that the anti-ultraviolet effect remains stable in long-term use. Therefore, titanium dioxide microspheres coated with anti-ultraviolet absorbing aids are undoubtedly an ideal choice, which is widely used in many fields such as coatings and plastics. This innovative technology provides strong UV protection for materials and buildings, significantly improves their weather resistance, and also improves energy efficiency.

[0135] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that all equivalent structural changes made under the concept of the present invention and using the contents of the present invention specification and drawings should be covered within the scope of protection of the claims of the present invention.

Claims

1. Anti-ultraviolet acrylic resin thermal insulation coating for building exterior walls, characterized in that: The composition is calculated by weight: 30-60 parts of titanium dioxide microspheres coated with ultraviolet absorbing agent composite filler, 80-110 parts of acrylic emulsion, 40-90 parts of anhydrous ethanol, 5-12 parts of talc, 1-6 parts of color enhancer, 2-5 parts of film former, 1-3 parts of dispersant, 1-3 parts of defoamer, 0.5-2 parts of leveling agent, 0.5-2 parts of preservative, 1-3 parts of hydroxypropyl methylcellulose; The average size of the titanium dioxide microsphere-coated ultraviolet absorbing additive composite filler is in the range of 50 to 200 nm; The preparation method of the titanium dioxide microsphere-coated ultraviolet absorption aid composite filler is as follows: first, by weight, 10 to 20 parts of nitrophenol and 30 to 60 parts of 2-bromoethanol are mixed evenly in 50 to 100 parts of dichloromethane solvent, and reacted at 50 to 80° C. for 2 to 4 hours to generate an aromatic ether compound; then 10 to 40 parts of 2-chloroethanol are added and stirred thoroughly, and then 30 to 60 parts of titanium dioxide microspheres are added, and the mixture is reacted at 80 to 120° C. for 4 to 12 hours to generate 2-chloro-4-nitrophenyloxyethylmethylcyclohexane in hollow titanium dioxide microspheres; finally, the titanium dioxide microsphere-coated ultraviolet absorption aid composite filler is obtained after washing and vacuum drying; the mass ratio of the nitrophenol, 2-bromoethanol and 2-chloroethanol is 1:3: (1 to 2); The preparation method of the titanium dioxide microspheres is as follows: 10-20 parts of fructose and 2-6 parts of sodium dodecyl sulfate are placed in 20-40 parts of a mixed solution of water and anhydrous ethanol in a volume ratio of 1:1, stirred evenly, placed in a high-pressure reactor, hydrothermally reacted at 160-250° C. for 12-24 hours, washed, filtered, and vacuum dried after cooling to obtain carbon hollow microspheres; 20-40 parts of carbon hollow microspheres, 5-10 titanium salts, and 2-6 parts of hexadecyl polyoxyethylene ether are dissolved in 100 parts of anhydrous ethanol, stirred evenly, placed in a high-pressure reactor, hydrothermally reacted at 120-160° C. for 6-12 hours, and then naturally cooled, filtered, washed, and dried to obtain titanium-containing compound-coated carbon hollow microspheres; finally, calcined at 500-600° C. for 2-4 hours in an air atmosphere to finally obtain titanium dioxide microspheres with a hollow structure; the titanium salt is a mixture of one or more of sodium titanate and potassium titanate; The preparation method of the acrylic emulsion is as follows: by weight, 4 to 10 parts of acrylic acid, 5 to 10 parts of ethyl acrylate, 30 to 50 parts of anhydrous ethanol and 3 to 6 parts of sodium dodecylbenzene sulfonate are stirred uniformly to form a mixed solution, and then 2 to 4 parts of ammonium persulfate are added to form an acrylic emulsion.

2. The anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls according to claim 1, characterized in that: The film-forming agent is a mixture of one or more of lauryl alcohol ester and polyethyl acrylate.

3. The anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls according to claim 1, characterized in that: The dispersant is polyethylene glycol.

4. The anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls according to claim 1, characterized in that: The defoamer is fatty alcohol polyoxyethylene ether.

5. The anti-ultraviolet acrylic resin heat-insulating coating for building exterior walls according to claim 1, characterized in that: The leveling agent is polydimethylsiloxane; The preservative is benzoic acid.

Citation Information

Cited By

  • Anti-ultraviolet acrylic resin coating and preparation method thereof

    CN121203479A

  • High-adhesion anti-ultraviolet acrylic coating for PC glass plate and preparation method of high-adhesion anti-ultraviolet acrylic coating

    CN121379268A