A method for prefilming an industrial recirculating cooling water system and use thereof
By using the nanobubble method for pre-filming treatment, the problems of environmental pollution and corrosion in traditional pre-filming treatment are solved, achieving a highly efficient pre-filming effect without secondary pollution and recycling of tailwater, thus reducing treatment costs.
Patent Information
- Application Number
- CN202410006452.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-03
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-03
AI Technical Summary
Existing pre-filming treatment methods for industrial circulating cooling water systems have environmental pollution problems. In particular, traditional pre-filming agents have high phosphorus content, which leads to high wastewater treatment costs and is harmful to the environment. Furthermore, traditional methods cannot effectively inhibit metal corrosion.
The nanobubble method is used for pre-filming treatment. Stable bubbles of 50-200 nm are formed in the circulating cooling water system by a nanobubble generator. Combined with a thermocouple heating device, the temperature is maintained at 70-80℃ for 60-100 hours of pre-filming treatment. The effluent can be recycled or discharged directly.
It achieves pre-filming treatment without secondary pollution, reduces the burden of wastewater treatment, improves the pre-filming effect, inhibits metal corrosion, and reduces phosphorus emissions in the effluent.
Smart Images

Figure CN117987816B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of industrial circulating cooling water pipeline treatment, specifically relating to a pre-filming method for industrial circulating water systems and its application. Background Technology
[0002] Pre-filming treatment is a necessary step in industrial circulating cooling water systems before commissioning, during maintenance, and after cleaning. After chemical cleaning, the metal surface is extremely reactive and prone to initial corrosion with a high corrosion rate. Pre-filming passivation treatment is urgently needed to form a corrosion-resistant protective film on the reactive metal surface, slowing down the erosion of the circulating water pipes by corrosive ions in the water during subsequent operation. Pre-filming treatment is crucial for extending pipe life and ensuring the stable operation of the circulating water system. Without pre-filming treatment, pipes may explode, perforate, or even become unusable, posing a serious threat to production safety.
[0003] Currently, pre-filming treatment is widely used in circulating cooling water systems by adding pre-filming agents. A common formulation is a combination of polyphosphate and zinc salt. While this method yields good pre-filming results, polyphosphate decomposes into orthophosphate during operation, causing a sharp increase in phosphorus and zinc content in the discharged wastewater. Long-term use can easily lead to eutrophication and environmental pollution. For example, patent CN1202028C discloses a pre-filming agent composed of phosphoric acid, zinc dihydrogen phosphate, a carboxylic acid-containing copolymer, organophosphonic acid, and benzotriazole. This pre-filming agent has a high phosphorus content, which significantly restricts the discharge of pre-filming effluent, and long-term use poses a significant environmental hazard.
[0004] To reduce environmental pollution, the use of low-phosphorus / phosphorus-free pre-filming agent formulations is gradually increasing. For example, pre-filming agents with polyepoxysuccinic acid (PESA) and polyaspartic acid (PASP) as main components are environmentally friendly and biodegradable, but their pre-filming performance is relatively low, often failing to meet usage requirements. During long-term use, the system experiences rapid corrosion, resulting in poor stable operation of circulating water pipelines. For instance, patent CN106011818B discloses a pre-filming agent composed of maleic anhydride-acrylamide-hydroxyethyl acrylate copolymer, polyaspartic acid, zinc sulfate, and hydroxyethylidene diphosphonic acid. Although this pre-filming agent has a low phosphorus content, it is not a completely phosphorus-free formulation and does not achieve true environmental friendliness. Furthermore, when using this pre-filming agent, the copper sulfate color development time is below 85 seconds, significantly lower than the phosphorus-containing formulation in patent CN1202028C (where the copper sulfate color development time is above 150 seconds), indicating that this formulation has lower pre-filming performance.
[0005] Typically, the wastewater after pre-filming needs to be treated for sewage discharge. This type of wastewater has a very large volume and high treatment costs. Therefore, there is an urgent need to develop an environmentally friendly pre-filming method that allows the wastewater to be recycled or directly discharged to solve the sewage discharge problem of industrial circulating water systems. Summary of the Invention
[0006] The present invention aims to provide a novel pre-filming method for industrial circulating cooling water systems—the nanobubble method for pre-filming treatment. Compared with traditional pre-filming methods, nanobubble pre-filming does not produce secondary pollution, is chemically harmless and environmentally friendly, and the resulting wastewater can be recycled or directly discharged.
[0007] The technical solution provided by this invention is as follows:
[0008] A pre-filming method for an industrial circulating cooling water system includes the following steps: pumping industrial circulating cooling water into a nanobubble generator, wherein the air source of the nanobubble generator is gas from a gas compressor, forming a high-pressure gas-water mixture and making the gas in a supersaturated dissolved state; releasing the gas in the form of nanobubbles into the circulating cooling water system through a release device and retaining it for 60-100 hours to perform pre-filming treatment on the industrial circulating cooling water system.
[0009] Furthermore, the nanobubbles are stable bubbles with a diameter of 50-200 nm.
[0010] Furthermore, the air source for the nanobubble generator is any one or more of air, nitrogen, and carbon dioxide.
[0011] Furthermore, the intake air pressure of the nanobubble generator is set as follows: P = k p,gas *μ gas *10 -6 Where P is the intake pressure, in MPa and kJ / m³. p,gas This is the pressure coefficient, with a value ranging from 4000 to 8000 Pa·ml·units. -1 μ gas The number density of nanobubbles ranges from 100 to 200 per ml. -1 ;
[0012] Furthermore, the air intake flow rate of the nanobubble generator is set as follows: V = k v,gas / μ gas Where V is the intake airflow rate, in ml / min, and k v,gas The flow coefficient, with a value ranging from 5000 to 6000 particles / min, is μ. gas The number density of nanobubbles ranges from 100 to 200 per ml. -1 ;
[0013] Furthermore, in order to maintain the long-term stable existence of nanobubbles, an electrocoupler heating device is installed in the circulating cooling water storage tank of the present invention to heat the inlet water of the nanobubble generator. The temperature range is set to 70-80℃. The specific reasons are as follows:
[0014] The size of nanobubbles is a key factor in maintaining their long-term stability; smaller nanobubbles are more likely to remain stable in solution. In circulating cooling water systems, a significant temperature difference exists between the inlet and outlet of the heat exchanger, and temperature is a crucial factor affecting the nanobubble size distribution. Studies show that as water temperature increases, the viscosity, density, and surface tension of the solution decrease. Larger nanobubbles are more likely to rise to the gas-liquid interface and collapse, thus the average particle size of nanobubbles in water gradually decreases and becomes more concentrated. At 30℃, the nanobubble size is concentrated at approximately 348 nm; at 50℃, it is concentrated at approximately 169 nm; and at 70℃, it is concentrated at approximately 45 nm. To maintain the long-term stability of nanobubbles and ensure a certain concentration of small-sized nanobubbles in the solution, this invention sets the temperature range to 70-80℃.
[0015] Furthermore, the liquid to gas flow ratio entering the nanobubble generator is 8 to 12:1.
[0016] Furthermore, the pre-filming time of the industrial circulating cooling water is set to 60-100 hours.
[0017] Furthermore, after the pre-filming is completed, some of the wastewater is transported back to the circulating cooling water storage tank through pipelines for the next nanobubble preparation, while the remaining wastewater is discharged directly.
[0018] Furthermore, after the pre-filming is completed, 90% of the tailwater from the circulating cooling water is discharged directly, and 10% is returned to the circulating cooling water storage tank via a return pump.
[0019] The present invention also provides the application of the above-mentioned pre-filming method for industrial circulating cooling water systems in reducing phosphorus emissions from the tailwater after pre-filming treatment of industrial circulating cooling water systems.
[0020] This invention provides a novel pre-filming method for industrial circulating cooling water systems. Specifically, industrial circulating cooling water is stored in a tank (the tank is equipped with an electrocouple heating device to maintain the inlet water temperature between 70-80°C) and pumped into a nanobubble generator. The gas source is gas from a gas compressor. The two form a high-pressure gas-water mixture in the nanobubble generator, and the gas is in a supersaturated dissolved state. Then, the gas is released into the circulating cooling water system in the form of nanobubbles through a release device. The nanobubbles undergo pre-filming treatment in the system. After pre-filming, part of the wastewater is transported back to the circulating cooling water storage tank through a pipeline for the next nanobubble preparation, and the remaining wastewater is directly discharged, thus solving the sewage discharge problem of industrial circulating cooling water systems.
[0021] Nanobubbles, typically stable bubbles with a diameter of 50-200 nm in liquids, possess advantages over ordinary micron-sized bubbles, including high oxygen mass transfer efficiency, hydroxyl radical cavitation formation, large specific surface area, long residence time in water, zero secondary pollution, and high stability. Unlike ordinary micron-sized bubbles that readily interact with Cl- in water to accelerate the corrosion of metal pipes, nanobubbles can act as a special "passivation film-type corrosion inhibitor," forming a passivation film on the metal surface to inhibit corrosion. The specific principle is as follows:
[0022] First, microbubbles can significantly influence fluid flow along the surface of hydrophobic microstructures by altering the frictional force of the liquid. This influence is typically expressed as the slip length of the flowing liquid at the solid interface; the lower the resistance at the interface, the greater the slip length. Experiments show that the slip length of water on a hydrophobic surface is usually less than 100 nm, while in the presence of nanobubbles, the slip length can reach 10 μm. Furthermore, experiments demonstrate that nanobubbles can persist for months, rather than the theoretically expected milliseconds. Due to their small size, nanobubbles possess low buoyancy, and their rising speed is very slow because their motion is controlled by random Brownian motion, allowing them to exist as surface nanobubbles (surface pinning). Surface nanobubbles can transform the solid-liquid interface from a two-phase contact to a three-phase contact. The nanobubbles are fixed and remain on rough surfaces for extended periods, which not only promotes increased slip length but also allows them to act as "bubble pads" covering metal surfaces, separating the metal from the fluid in the circulating cooling water and preventing further corrosion.
[0023] Furthermore, the zeta potential of nanobubbles exhibits an S-shaped distribution with pH value. They carry a positive charge in acidic solutions and a negative charge at normal pH values. The charged surfaces generally tend to adsorb counterions from the medium, thus forming a stable electrical double layer. Therefore, when nanobubbles interact with scale particles (such as Ca²⁺), they can form a stable electrical double layer. 2+ When simultaneously charged, nanobubbles with the opposite charge to the scale particles may adhere to the scale particles, aiding in their flotation and preventing multi-layered scale deposition on the metal surface. The specific process is as follows: 1) In the initial stage of contact between the nanobubbles and the metal surface, a bubble layer rapidly forms. This bubble layer effectively reduces the direct contact area between the metal surface and corrosion ions, mitigating pitting corrosion; 2) The nanobubble layer increases the DO concentration near the metal surface, and the ·OH generated by bubble collapse can directly act on the metal surface, promoting the formation of a passivation film; 3) The collapse of the bubble layer can cause Ca in the boundary layer to... 2+Increased concentration promotes the rapid formation of calcium carbonate scale film, resulting in a hydrophobic calcium carbonate scale film that covers the passivation film. The formation of the passivation film and the scale inhibition film creates a double layer of protection on the metal surface; 4) The outer layer of the calcium scale film adsorbs air bubbles. The presence of the bubble layer reduces friction, increases slip length, effectively inhibits the thickening of the calcium carbonate scale film, and suppresses multilayer deposition; 5) Nanobubbles present in the water can further adsorb scale cations due to the double electric layer principle, reducing scale precipitation. Specific mechanisms are as follows: Figure 1 As shown.
[0024] Furthermore, compared with traditional high-performance chemical pre-filming agents, nanobubbles can maintain stability and effectiveness at higher temperatures and pressures, and can be applied to a variety of metal materials and flow patterns. This avoids many problems with chemical pre-filming agents, which are limited by specific metal materials or flow characteristics. For example, acidic pre-filming agents tend to severely corrode metals such as iron and copper; alkaline pre-filming agents are highly corrosive to galvanized pipes and aluminum heat exchangers; and traditional pre-filming methods are not suitable for jet-like fluids.
[0025] Beneficial effects
[0026] Traditional pre-filming methods often use a phosphorus-based combination formula of "polyphosphate + zinc salt". This method produces wastewater with high phosphorus content, which can easily lead to eutrophication and environmental pollution with long-term use. Therefore, it cannot be directly discharged and requires additional treatment processes, increasing the difficulty and cost of wastewater treatment. In contrast, the nanobubble pre-filming method provided by this invention does not require the addition of additional chemical agents, does not produce secondary pollution in the discharged wastewater, is chemically harmless, environmentally friendly, easy to use, and low in cost.
[0027] Traditional pre-filming methods result in a large volume of wastewater discharge and a heavy burden on effluent treatment. The pre-filming method provided by this invention can recycle effluent or discharge it directly, greatly reducing the burden of subsequent treatment.
[0028] The novel pre-filming method provided by this invention achieves good results. The nanobubbles possess characteristics such as high oxygen mass transfer efficiency, hydroxyl radical cavitation formation, large specific surface area, long residence time in water, and zero secondary pollution. They not only promote an increase in slip length, but the surface nanobubbles also act like "bubble pads" covering the metal surface, separating the metal from the fluid in the circulating cooling water and preventing further corrosion. Furthermore, the negatively charged nanobubbles can adsorb scale particles with opposite charges, forming a stable electric double layer, which facilitates the flotation of scale particles and prevents multi-layer deposition of scale on the metal surface.
[0029] Compared with traditional high-performance chemical pre-filming agents, nanobubbles can maintain stability and effectiveness at higher temperatures and pressures, and can be applied to a variety of metal materials and flow patterns, avoiding the problem that many chemical pre-filming agents are limited by specific metal materials or flow characteristics. Attached Figure Description
[0030] Figure 1 This is a diagram illustrating the mechanism of nanobubble interaction.
[0031] Figure 2 This is a flow chart of the nanobubble pre-filming process. Detailed Implementation
[0032] Example 1:
[0033] The water quality information table for the open-loop circulating cooling water system of an integrated circuit factory in Wuxi is as follows:
[0034]
[0035] The pre-filming treatment using the method of this invention comprises the following specific steps:
[0036] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 75°C. Set the inlet pressure of the nanobubble generator to 0.4MPa and the inlet flow rate to 30mL / min using the formula of inlet pressure and inlet flow rate.
[0037] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 10:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0038] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0039] (4) The corroded carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 92 seconds.
[0040] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.05 ppm.
[0041] Example 2:
[0042] The water quality information table for the open-loop circulating cooling water system of an integrated circuit factory in Yantai is as follows:
[0043]
[0044] The pre-filming treatment using the method of this invention comprises the following specific steps:
[0045] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 75°C. Set the inlet pressure of the nanobubble generator to 0.4MPa and the inlet flow rate to 30mL / min using the formula of inlet pressure and inlet flow rate.
[0046] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 10:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0047] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0048] (4) The corroded carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 87 seconds.
[0049] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.075 ppm.
[0050] Comparative Example 1:
[0051] The pre-filming method of Comparative Example 1 is basically the same as that of Example 1, except that a nanobubble generator is not used in Comparative Example 1. After the circulating cooling water and gas are mixed, they are directly introduced into the circulating cooling water system through the circulating water pump.
[0052] The specific steps are as follows:
[0053] (1) Store the effluent from the circulating cooling water system in a storage tank, turn on the thermocouple heating device and set the temperature to 75°C, adjust the ratio of the effluent flow rate of the circulating cooling water storage tank to the gas flow rate of the gas compressor to 10:1, and turn on the circulating water pump. Both enter the circulating cooling water system through the water pump.
[0054] (2) The corrosion carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 5s, which was lower than the national standard of ≥7s, indicating that the pre-filming failed. The total phosphorus content of the tailwater was measured to be 1.15ppm.
[0055] By comparing Comparative Example 1 with Example 1, it can be seen that when the nanobubble solution is used for pre-filming treatment, the color change time of copper sulfate is much greater than the value specified in the national standard, indicating that nanobubbles can effectively perform pre-filming treatment.
[0056] Comparative Example 2:
[0057] The pre-filming method of Comparative Example 2 is basically the same as that of Example 1. The only difference is that Comparative Example 2 does not use nanobubble solution for pre-filming, but uses the traditional combination of "polyphosphate + zinc salt" for pre-filming. The specific components are: polyphosphate: zinc chloride: organic acid = 10:3:10.
[0058] The specific steps are as follows:
[0059] (1) Add the prepared pre-filming agent to the circulating cooling water system at a concentration of 100-200 mg pre-filming agent / L water, slowly heat the system temperature to 75°C, and start the pre-filming treatment. The pre-filming time is set to 72h.
[0060] (2) The corrosion carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 108s, which is much higher than the national standard of ≥7s. The total phosphorus content of the tailwater was measured to be 2.13ppm.
[0061] Comparing Comparative Example 2 with Example 1, it can be seen that when using a phosphorus- and zinc-containing pre-filming agent for pre-filming treatment, the color change time of copper sulfate is increased by about 15% compared to the nanobubble method, but the phosphorus content of the effluent is greatly increased. The phosphorus content of the effluent after pre-filming by the nanobubble method is reduced by 97.6% compared to the phosphorus content of the effluent after pre-filming by the phosphorus- and zinc-containing pre-filming agent addition method. This indicates that the nanobubble pre-filming method can greatly reduce the effluent treatment pressure and is chemically harmless and environmentally friendly.
[0062] Comparative Example 3:
[0063] The pre-filming method of Comparative Example 3 is basically the same as that of Example 1, except that the temperature of the thermocouple heating device in the circulating cooling water storage tank of Comparative Example 3 is set to 30°C. The specific steps are as follows:
[0064] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 30℃. Set the inlet pressure of the nanobubble generator to 0.4MPa and the inlet flow rate to 30mL / min using the formula of inlet pressure and inlet flow rate.
[0065] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 10:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0066] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0067] (4) The corroded carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 68 seconds.
[0068] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.12 ppm.
[0069] By comparing Comparative Example 3 with Example 1, it can be seen that when the influent temperature is reduced from 75°C to 30°C, the copper sulfate color change time decreases by about 26%, and the phosphorus content in the effluent increases by 140%. This indicates that temperature has a significant impact on the pre-filming effect in the nanobubble pre-filming method. After the temperature is reduced, the pre-filming effect decreases and the phosphorus content in the effluent increases.
[0070] Comparative Example 4:
[0071] The pre-filming method in Comparative Example 4 is basically the same as that in Example 1, except that the pressure coefficient of the nanobubble generator in Comparative Example 4 is not within the reference range (P = k). p,gas *μ gas *10 -6 Where P is the intake pressure, in MPa and kJ / m³. p,gas This is the pressure coefficient, with a value ranging from 4000 to 8000 Pa·ml·units. -1 μ gas The number density of nanobubbles is a custom value, with a reference range of 100-200 bubbles per ml. -1 The pressure coefficient is set to 2000 Pa·ml·unit. -1 The intake pressure is 0.2 MPa.
[0072] The specific steps are as follows:
[0073] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 30℃. Set the inlet pressure of the nanobubble generator to 0.2MPa and the inlet flow rate to 30mL / min using the formula of inlet pressure and inlet flow rate.
[0074] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 10:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0075] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0076] (4) The corroded carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 65 seconds.
[0077] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.15 ppm.
[0078] By comparing Comparative Example 4 with Example 1, it can be seen that when the inlet pressure coefficient is not within the range, and the inlet pressure is reduced from 0.4 MPa to 0.2 MPa, the copper sulfate color change time decreases by about 29%, and the phosphorus content in the tailwater increases by 200%. This indicates that the inlet pressure of the nanobubble generator in the nanobubble pre-filming method has a significant impact on the pre-filming effect. After the pressure is reduced, the pre-filming effect decreases and the phosphorus content in the tailwater increases.
[0079] Comparative Example 5:
[0080] The pre-filming method in Comparative Example 5 is basically the same as that in Example 1, except that the flow coefficient of the nanobubble generator in Comparative Example 5 is not within the reference range (V = k). v,gas / μ gas Where V is the intake airflow rate, in ml / min, and k v,gas The flow coefficient, with a value ranging from 5000 to 6000 particles / min, is μ. gas The number density of nanobubbles is a custom value, with a reference range of 100-200 bubbles per ml. -1 ;) Configure the flow rate coefficient to 3000 Pa·ml·cell -1 The intake flow rate is 15 mL / min.
[0081] The specific steps are as follows:
[0082] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 30℃. Set the inlet pressure of the nanobubble generator to 0.4MPa and the inlet flow rate to 15mL / min using the formula of inlet pressure and inlet flow rate.
[0083] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 10:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0084] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0085] (4) The corroded carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 72 seconds.
[0086] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.13 ppm.
[0087] By comparing Comparative Example 5 with Example 1, it can be seen that when the inlet flow rate coefficient is not within the range, and the inlet flow rate is reduced from 30 mL / min to 15 mL / min, the copper sulfate color change time decreases by about 21.7%, and the phosphorus content in the tailwater increases by 160%. This indicates that the inlet flow rate of the nanobubble generator in the nanobubble pre-filming method has a significant impact on the pre-filming effect. After the flow rate is reduced, the pre-filming effect decreases and the phosphorus content in the tailwater increases.
[0088] Comparative Example 6:
[0089] The pre-filming method of Comparative Example 6 is basically the same as that of Example 1, except that the pre-filming time in Comparative Example 6 is reduced from 72h to 50h.
[0090] The specific steps are as follows:
[0091] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 75°C. Set the inlet pressure of the nanobubble generator to 0.4MPa and the inlet flow rate to 30mL / min using the formula of inlet pressure and inlet flow rate.
[0092] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 10:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0093] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0094] (4) The corroded carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 50 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 60 seconds.
[0095] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.23 ppm.
[0096] By comparing Comparative Example 6 with Example 1, it can be seen that when the pre-filming time is reduced from 72h to 50h, the copper sulfate color change time decreases by about 34.8%, and the phosphorus content in the effluent increases by 360%. This indicates that the pre-filming time in the nanobubble pre-filming method has a significant impact on the pre-filming effect. When the time is reduced, the pre-filming effect decreases and the phosphorus content in the effluent increases.
[0097] Comparative Example 7:
[0098] The pre-filming method of Comparative Example 7 is basically the same as that of Example 1, except that the ratio of the flow rate of the circulating cooling water tank to the flow rate of the gas compressor in Comparative Example 7 is 12:1.
[0099] The specific steps are as follows:
[0100] (1) Store the effluent from the circulating cooling water system in a storage tank, and turn on the thermocouple heating device to set the temperature to 75°C. Set the inlet pressure of the nanobubble generator to 0.4MPa and the inlet flow rate to 30mL / min using the formula of inlet pressure and inlet flow rate.
[0101] (2) Adjust the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor to 12:1, and turn on the circulating water pump. The two enter the nanobubble generator through the water pump to form a high-pressure gas-water mixture.
[0102] (3) The gas is in a supersaturated dissolved state in the nanobubble generator and is released into the circulating cooling water system through the release device to form a nanobubble solution for pre-filming treatment.
[0103] (4) The corrosion carbon steel test piece was hung in the circulating cooling water pool to test the pre-filming effect. After 72 hours, the test piece was taken out and a copper sulfate solution titration test was performed. The color change time was 75 seconds.
[0104] (5) 90% of the circulating cooling water tailwater after the pre-filming is completed is discharged directly, and 10% is returned to the circulating cooling water storage tank through a return pump. The total phosphorus content of the tailwater is measured to be 0.10 ppm.
[0105] By comparing Comparative Example 7 with Example 1, it can be seen that when the ratio of the outflow rate of the circulating cooling water storage tank to the outflow rate of the gas compressor is reduced from 10:1 to 12:1, the color change time of copper sulfate decreases by about 18.5%, and the phosphorus content of the tailwater increases by 100%. This indicates that the ratio of the outflow rate to the outflow rate in the nanobubble pre-filming method has a significant impact on the pre-filming effect. When the ratio decreases, the pre-filming effect decreases and the phosphorus content of the tailwater increases.
Claims
1. The application of a pre-filming method for industrial circulating cooling water systems in reducing phosphorus emissions from the tailwater after pre-filming treatment of industrial circulating cooling water systems, characterized in that, The pre-filming method for the industrial circulating cooling water system includes the following steps: A thermocouple heating device is installed in the circulating cooling water storage tank to heat the inlet water of the nanobubble generator, with the temperature range set to 70-80℃. The industrial circulating cooling water is pumped into the nanobubble generator, where the air source is gas from a gas compressor, forming a high-pressure gas-water mixture and placing the gas in a supersaturated dissolved state. The gas-water mixture is then released through a release device, releasing the gas in the form of nanobubbles into the circulating cooling water system and retaining it for 60-100 hours to perform pre-filming treatment on the industrial circulating cooling water system. After pre-filming, a portion of the wastewater is re-transported through a pipeline to the circulating cooling water storage tank for the next nanobubble preparation, while the remaining wastewater is directly discharged.
2. The application according to claim 1, characterized in that, The nanobubbles are stable bubbles with a diameter of 50-200 nm.
3. The application according to claim 1, characterized in that, The air source for the nanobubble generator can be any one or more of air, nitrogen, and carbon dioxide.
4. The application according to claim 1, characterized in that, The inlet air pressure of the nanobubble generator is set as follows: P=k p,gas *µ gas *10 -6 Where P is the intake pressure, in MPa and kJ / m³. p,gas This is the pressure coefficient, with a value ranging from 4000 to 8000 Pa·ml·units. -1 µ gas The number density of nanobubbles ranges from 100 to 200 per ml. -1 .
5. The application according to claim 1, characterized in that, The air intake flow rate of the nanobubble generator is set as follows: V=k v,gas / µ gas Where V is the intake airflow rate, in ml / min, and k v,gas The flow coefficient, ranging from 5000 to 6000 particles / min, µ gas The number density of nanobubbles ranges from 100 to 200 per ml. -1 .
6. The application according to claim 1, characterized in that, The liquid to gas flow rate ratio entering the nanobubble generator is 8~12:
1.
7. The application according to claim 1, characterized in that, After the pre-filming is completed, 90% of the tailwater of the circulating cooling water is discharged directly, and 10% is returned to the circulating cooling water storage tank through the return pump.
Citation Information
Patent Citations
A pre-film agent for pre-film treatment of circulating cooling water system
CN106011818B
Pretreatment filming agent and pretreatment filming method for circulating cooling water system
CN1202028C