Anti-ultraviolet polyester composite yarn and its processing technology
By using a combination of anti-ultraviolet agent and nanofiller in polyester fibers, the UV resistance and physical and mechanical properties of polyester composite wires are improved, and the problem of insufficient anti-ultraviolet properties of traditional polyester filaments is solved, achieving long-lasting, stable and efficient protection Effect.
Patent Information
- Application Number
- CN202410203642.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-02-23
AI Technical Summary
Traditional polyester filaments have poor performance in UV resistance. The existing additives of UV resistance polyester filaments are prone to migration or fall off, resulting in poor durability of UV resistance and may have a negative impact on physical and mechanical properties and cannot meet the functions. demand for sexual textiles.
The anti-ultraviolet agent 2-(2ˊ-hydroxy-5ˊ-methylphenyl)benzotriazole was mixed with polyester slices, and the ultraviolet absorber UV-328 was combined on the spinning surface by impregnation treatment, and the nanometers were combined. Fillers such as nanotitanium dioxide and nanozinc oxide form a reflective layer or scattering layer, improving the UV resistance and physical and mechanical properties of spinning.
The polyester composite wire has achieved significant improvement in UV resistance and physical and mechanical properties, maintaining long-term stability and efficient protection, while avoiding the negative impact of additives on fiber performance.
Smart Images

Figure BDA0004712313720000141
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyester yarns, and in particular to anti-ultraviolet polyester composite yarns and a processing technology. Background Art
[0002] Polyester yarn has been widely used in textile and industrial fields due to its excellent strength and modulus, excellent heat and wear resistance, good shape retention, easy washing and drying, and low cost. As the chemical fiber with the largest output and the most extensive application, polyester yarn has an irreplaceable position in the market.
[0003] However, with the increasing demand for functional textiles in modern society, especially in the fields of outdoor clothing, car interiors, household items, etc., fiber materials with excellent UV resistance are increasingly attracting people's attention. Traditional polyester filaments have poor UV resistance and cannot meet people's demand for efficient protection. In addition, the existing UV-resistant polyester filaments mainly achieve UV resistance by adding UV absorbers or reflectors. Although these methods can improve the UV resistance of polyester filaments to a certain extent, there are problems such as easy migration of absorbers and easy shedding of reflectors, resulting in poor durability of UV resistance. In addition, the addition of these additives may also have a negative impact on the physical and mechanical properties of polyester filaments.
[0004] Therefore, a novel anti-ultraviolet polyester composite yarn and its processing technology are developed to solve the problems existing in the prior art. Based on this, the present invention develops a polyester composite yarn with excellent anti-ultraviolet performance and its processing technology, which has excellent anti-ultraviolet performance, long-term stability and good physical and mechanical properties, meeting the needs of functional textiles in different fields. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-ultraviolet polyester composite yarn and a processing technology to improve the anti-ultraviolet performance of the polyester filament while maintaining its excellent physical and mechanical properties and processing performance.
[0006] In a first aspect, the present invention provides a process for processing UV-resistant polyester composite yarn, the steps comprising:
[0007] S1. Pre-spinning treatment: drying the poly(trimethylene terephthalate) slices and the polyethylene terephthalate slices at 120-140° C. until the moisture content is less than 50 ppm for later use;
[0008] S2, melt spinning: the pre-treated slices are mixed with the anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and the additives, melt-spinned at 200-240°C, and cooled and formed by side blowing;
[0009] S3, composite treatment: put the cooled and formed spinning into the treatment liquid for immersion treatment, the mass ratio of spinning to treatment liquid is 1: (45-50);
[0010] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0011] Furthermore, the intrinsic viscosity of the poly(trimethylene terephthalate) slice is 1.05-1.32 dL / g; and the intrinsic viscosity of the poly(ethylene terephthalate) slice is 0.62-0.71 dL / g.
[0012] Furthermore, the weight ratio of the poly(trimethylene terephthalate) slice, the polyethylene terephthalate slice, the anti-ultraviolet agent and the auxiliary agent is (40-45):(26-32):(4-6):(3-5).
[0013] Furthermore, the auxiliary agent includes an antioxidant, a dispersant and a nanofiller in a weight ratio of (3-7): (4-6): (10-12).
[0014] Furthermore, the antioxidant includes antioxidant 168 and antioxidant 1010 in a mass ratio of (1-2):(1-4).
[0015] Furthermore, the dispersant is polyvinyl pyrrolidone with a molecular weight of 30,000-50,000; and the nano filler includes nano titanium dioxide and / or nano zinc oxide.
[0016] Furthermore, the side-blowing cooling air temperature is 30-32° C., and the side-blowing air speed is 0.5-0.8 m / s.
[0017] Furthermore, the treatment liquid includes a surfactant TX-10, an ultraviolet absorber UV-328, and a dispersant SMA1440F in a weight ratio of (2-3): (4-6): (0.5-1).
[0018] Furthermore, the dipping method is two dipping and two rolling at room temperature, and the rolling rate is 75-80%. After the dipping is completed, it is pre-baked at 60-80°C for 5-8 minutes and baked at 120-160°C for 1-5 minutes.
[0019] In a second aspect, the present invention provides an anti-ultraviolet polyester composite yarn, which is prepared by the aforementioned processing technology.
[0020] The beneficial effects of the present invention are:
[0021] (1) The present invention uses an anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and polyester chips for mixed spinning, and then uses an immersion treatment method to compound an ultraviolet absorber UV-328 on the spinning surface; in addition, the nanofiller added in the present invention can effectively fill the molecular pores of the composite spinning, and on the basis of improving the mechanical properties of the spinning, it also effectively improves the anti-ultraviolet performance of the spinning;
[0022] (2) 2-(2ˊ-Hydroxy-5ˊ-methylphenyl)benzotriazole and UV-328 mainly work by absorbing ultraviolet rays and converting them into heat or other forms of energy, and can be evenly distributed inside the fiber. However, this organic anti-ultraviolet agent will gradually decompose and become ineffective due to factors such as temperature and light. In the present invention, not only the two are coordinated to improve the anti-ultraviolet performance, but also the anti-ultraviolet agent is compounded by configuring the treatment liquid to impregnate the spinning, thereby effectively improving the composite fastness of the anti-ultraviolet agent and the spinning;
[0023] (3) The present invention uses nano titanium dioxide and / or nano zinc oxide as nano fillers, which can form a reflective layer on the surface of the polyester fiber to reflect ultraviolet rays back or reduce the penetration of ultraviolet rays by scattering. In addition, the stability of the inorganic filler is not high. The impregnation method of the present invention is two impregnations and two rollings at room temperature, and the rolling rate is 75-80%. After the impregnation is completed, it is pre-baked at 60-80°C for 5-8 minutes and baked at 120-160°C for 1-5 minutes. This impregnation method also improves the composite fastness of the nano filler. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] This embodiment provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0027] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0028] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0029] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0030] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0031] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0032] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0033] Example 2
[0034] This embodiment provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0035] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.14 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.64 dL / g at 125° C. until the water content is less than 50 ppm for later use;
[0036] S2, melt spinning: 43 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 4 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 5 parts of auxiliary agent are mixed, melt-spinned at 200°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 30°C, and the side-blowing wind speed is 0.5m / s;
[0037] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (3): (4): (10); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1): (1); the dispersant is polyvinyl pyrrolidone with a molecular weight of 30,000; the nanofiller comprises nano titanium dioxide;
[0038] S3, composite treatment: the cooled and formed spinning is placed in a treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 75%, after the immersion is completed, it is pre-baked at 60℃ for 8min and baked at 120℃ for 5min; the mass ratio of spinning to treatment liquid is 1:(45);
[0039] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (2):(4):(0.5);
[0040] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0041] Example 3
[0042] This embodiment provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0043] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.22 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.70 dL / g at 140° C. until the water content is less than 50 ppm for later use;
[0044] S2, melt spinning: 45 parts of pre-treated poly(trimethylene terephthalate) slices, 32 parts of polyethylene terephthalate slices, 6 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 5 parts of auxiliary agent are mixed, melt-spinned at 240°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 32°C, and the side-blowing wind speed is 0.8 m / s;
[0045] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (7): (6): (12); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (2): (1); the dispersant is polyvinyl pyrrolidone with a molecular weight of 50,000; the nanofiller comprises nano zinc oxide;
[0046] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 80%, after the immersion is completed, it is pre-baked at 80℃ for 8min and baked at 160℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(50);
[0047] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (3): (6): (1);
[0048] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0049] Example 4
[0050] This embodiment provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0051] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.24 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.68 dL / g at 125° C. until the water content is less than 50 ppm for later use;
[0052] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 27 parts of polyethylene terephthalate slices, 4 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 5 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0053] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (4): (12); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (2): (4); the dispersant is polyvinyl pyrrolidone with a molecular weight of 50,000; the nanofiller comprises nano titanium dioxide;
[0054] S3, composite treatment: the cooled and formed spinning is placed in a treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 80%, after the immersion is completed, it is pre-baked at 80℃ for 8min and baked at 160℃ for 4min; the mass ratio of spinning to treatment liquid is 1:(48);
[0055] The treatment liquid includes a surfactant TX-10, an ultraviolet absorber UV-328, and a dispersant SMA1440F in a weight ratio of (2):(6):(1);
[0056] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0057] Comparative Example 1
[0058] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0059] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0060] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0061] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0062] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0063] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0064] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0065] Comparative Example 2
[0066] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0067] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0068] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0069] The auxiliary agent includes an antioxidant and a dispersant in a weight ratio of (5): (5); the antioxidant includes antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000;
[0070] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0071] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0072] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0073] Comparative Example 3
[0074] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0075] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0076] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0077] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0078] S3, post-processing: the fibers obtained by spinning are stretched and shaped to obtain composite fibers.
[0079] Comparative Example 4
[0080] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0081] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0082] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0083] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0084] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0085] The treatment liquid includes a surfactant OP-10, an ultraviolet absorber UV-328, and a dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0086] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0087] Comparative Example 5
[0088] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0089] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0090] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0091] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0092] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0093] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-531 and dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0094] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0095] Comparative Example 6
[0096] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0097] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0098] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0099] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0100] S3, composite treatment: the cooled and formed spinning is placed in the treatment liquid for immersion treatment, the immersion method is two immersions and two rollings at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0101] The treatment liquid includes a surfactant TX-10, an ultraviolet absorber UV-P 2-(2ˊ-hydroxy-5ˊ-methylphenyl)benzotriazole and a dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0102] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0103] Comparative Example 7
[0104] This comparative example provides a processing technology for anti-ultraviolet polyester composite yarn, the steps comprising:
[0105] S1. Pre-spinning treatment: drying poly(trimethylene terephthalate) chips with an intrinsic viscosity of 1.21 dL / g and poly(ethylene terephthalate) chips with an intrinsic viscosity of 0.66 dL / g at 130° C. until the water content is less than 50 ppm for later use;
[0106] S2, melt spinning: 42 parts of pre-treated poly(trimethylene terephthalate) slices, 29 parts of polyethylene terephthalate slices, 5 parts of anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 4 parts of additives are mixed, melt-spinned at 220°C, and formed by side-blowing cooling; the side-blowing cooling air temperature is 31°C, and the side-blowing wind speed is 0.6 m / s;
[0107] The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (5): (5): (6); the antioxidant comprises antioxidant 168 and antioxidant 1010 in a weight ratio of (1.5): (2.5); the dispersant is polyvinyl pyrrolidone with a molecular weight of 40,000; the nanofiller comprises nano titanium dioxide and nano zinc oxide in a weight ratio of 1:1;
[0108] S3, composite treatment: the cooled and formed spinning is placed in a treatment liquid for immersion treatment, the immersion method is one immersion and one rolling at room temperature, each immersion time is 2.5 hours, the immersion is carried out under 350HZ ultrasonic conditions, and the rolling liquid rate is 78%, after the immersion is completed, it is pre-baked at 70℃ for 6min and baked at 140℃ for 3min; the mass ratio of spinning to treatment liquid is 1:(47);
[0109] The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (2.5):(5):(0.7);
[0110] S4, post-processing: the composite fiber is stretched and shaped to obtain the composite yarn.
[0111] The following performance tests were performed on the polyester filaments obtained in Examples 1 to 4 and Comparative Examples 1 to 7:
[0112] (1) Elongation at break: According to GB / T1040.2-2006, the breaking strength performance of the samples was tested;
[0113] (2) Anti-ultraviolet performance test: The composite yarn single filament fineness is 1.02 dtex, woven into a one-up-one-down plain woven fabric in accordance with GB / T18830-2009 “Evaluation of the anti-ultraviolet performance of textiles”.
[0114] The test results are shown in Table 1 below:
[0115] Table 1
[0116]
[0117] Finally, it should be noted that the above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A process for processing UV-resistant polyester composite yarn, characterized in that the steps include: S1. Pre-spinning treatment: drying the poly(trimethylene terephthalate) slices and the polyethylene terephthalate slices at 120-140° C. until the moisture content is less than 50 ppm for later use; S2, melt spinning: the pre-treated slices are mixed with the anti-ultraviolet agent 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and the additives, melt-spinned at 200-240°C, and cooled and formed by side blowing; S3, composite treatment: put the cooled and formed spinning into the treatment liquid for immersion treatment, the mass ratio of spinning to treatment liquid is 1: (45-50); S4, post-processing: stretching and shaping the composite treated fiber to obtain the composite yarn; The auxiliary agent comprises an antioxidant, a dispersant and a nanofiller in a weight ratio of (3-7): (4-6): (10-12); the nanofiller comprises nano titanium dioxide and / or nano zinc oxide; The treatment liquid includes surfactant TX-10, ultraviolet absorber UV-328 and dispersant SMA1440F in a weight ratio of (2-3): (4-6): (0.5-1); the dipping method is double dipping and double rolling at room temperature, and the rolling rate is 75-80%, and after the dipping is completed, it is pre-baked at 60-80°C for 5-8 minutes and baked at 120-160°C for 1-5 minutes.
2. The processing technology of the anti-ultraviolet polyester composite yarn according to claim 1, characterized in that: The intrinsic viscosity of the poly(trimethylene terephthalate) slice is 1.05-1.32 dL / g; the intrinsic viscosity of the polyethylene terephthalate slice is 0.62-0.71 dL / g.
3. The processing technology of the anti-ultraviolet polyester composite yarn according to claim 1, characterized in that: The weight ratio of the poly(trimethylene terephthalate) slice, the polyethylene terephthalate slice, the anti-ultraviolet agent and the auxiliary agent is (40-45): (26-32): (4-6): (3-5).
4. The processing technology of the anti-ultraviolet polyester composite yarn according to claim 1, characterized in that: The antioxidant includes antioxidant 168 and antioxidant 1010 in a mass ratio of (1-2):(1-4).
5. The processing technology of the anti-ultraviolet polyester composite yarn according to claim 1, characterized in that: The dispersant is polyvinyl pyrrolidone with a molecular weight of 30,000-50,000.
6. The processing technology of the anti-ultraviolet polyester composite yarn according to claim 1, characterized in that: The side-blowing cooling air temperature is 30-32° C., and the side-blowing air speed is 0.5-0.8 m / s.
7. Anti-ultraviolet polyester composite yarn, characterized in that: The invention is prepared by the processing technology described in any one of claims 1 to 6.
Citation Information
Patent Citations
Anti-ultraviolet polyester fibers and preparation method thereof
CN105088389A
Ultrafine denier polyester filaments and preparation method thereof
CN108193309A
Production process of anti-ultraviolet polyester low stretch yarns
CN110055615A
Process for preparing coloured flame retardant polyester fibre
WO2017066975A1
Dedicated polyester industrial yarn for marine hawsers and preparation method therefor