A method for preparing lithium ion sieve adsorbent
By doping transition metals in the manganese oxide ion sieve precursor and using crosslinking systems and multivariate copolymers, the stability and adsorption capacity of lithium ion sieve in high mineralization water is improved, and the lithium ion sieve in high mineralization is solved. The problem of poor stability in the water of hydration has achieved a more efficient lithium ion extraction effect.
Patent Information
- Application Number
- CN202310460984.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-26
AI Technical Summary
The existing lithium ion sieve adsorbents have poor stability in salt lake brine or underground brine or gas field water with high mineralization, and their adsorption capacity is not high, which limits their industrial applications.
The transition metal is doped into the manganese oxide ion sieve precursor by hydrothermal reaction method, and the obtained doped ion sieve H1.6 (Mn M)1.6O4 maintained the spinel structure, and passed the crosslinking system and multi-copolymer. Enhance the stability of the composite hydrogel, improve the valence state of manganese elements, inhibit the Jahn-Teller effect, and enhance the adsorption capacity and selectivity of lithium ions.
It improves the adsorption capacity and structural stability of lithium ions, enhances the selectivity of lithium ions, solves the problem of instability of lithium ion sieve in high mineralization water, and achieves more efficient lithium ion extraction.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium ion recovery, and in particular to a method for preparing a lithium ion sieve adsorbent. Background Art
[0002] In recent years, with the rapid development of mobile electronic devices and electric vehicles, the demand for batteries has continued to grow. As the "white oil" of the new era, lithium is used as the main raw material for lithium batteries. With the rapid growth in demand for new energy vehicles, the demand for lithium carbonate has exploded and the price has skyrocketed. It is estimated that the global demand for lithium in 2025 will be about 1.5 million tons (equivalent to 7.93 million tons of lithium carbonate, with a unit price of 200,000 yuan / ton, and an output value of about 158.6 billion), and the total market demand will grow at an annual rate of about 30%. At present, lithium products are mainly derived from lithium extraction from ores (spodumene, lithium mica, etc.) and salt lakes. However, this still cannot meet the demand for lithium in today's lithium battery industry. After exploration, it was found that lithium resources are also widely present in underground brine and gas field water. In order to extract lithium from the above four types of raw materials, it is almost always carried out under aqueous conditions. For lithium extraction in aqueous phase, the most critical thing is lithium adsorbent.
[0003] The spinel manganese oxide ion sieve adsorbent material has become one of the most promising adsorbent materials for lithium extraction due to its stable spinel structure and special three-dimensional tunnel structure, high adsorption capacity, good selectivity, good recyclability, low raw material cost and certain theoretical basis support. However, it is difficult to directly apply the ion sieve adsorbent powder material, and its stability is poor in highly mineralized salt lake brine, underground brine or gas field water. The adsorption rate and adsorption capacity need to be further improved, which limits the industrial application of this type of adsorbent. Summary of the invention
[0004] The main purpose of the present application is to provide a method for preparing a lithium ion sieve adsorbent, aiming to solve the technical problem of poor adsorption capacity of ion sieve adsorbents in the prior art.
[0005] To achieve the above object, the present application proposes a method for preparing a lithium ion sieve adsorbent, comprising the following steps:
[0006] The ion sieve precursor Li is prepared by using lithium-containing compounds and manganese salts as raw materials and doping with transition metal M by hydrothermal reaction. 1.6 (Mn M) 1.6 O4;
[0007] The above ion sieve precursor is subjected to acidification treatment to obtain ion sieve H 1.6 (Mn M) 1.6 O4;
[0008] Add the first crosslinking agent and the second crosslinking agent into water, heat and stir evenly to obtain a crosslinking system;
[0009] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0010] Adding a multi-component copolymer to the cross-linking system, adding the cross-linked copolymer to the chitosan solution, and then adding the ion sieve, stirring and mixing to obtain a composite hydrogel;
[0011] After the composite hydrogel is dried, an adsorbent containing a lithium ion sieve is obtained.
[0012] Optionally, the lithium-containing compound is lithium hydroxide monohydrate; and the manganese salt is manganese carbonate.
[0013] Optionally, the above transition metals include cobalt and copper.
[0014] Optionally, the ion sieve precursor Li is prepared by the hydrothermal reaction method. 1.6 (Mn M) 1.6 The steps of O4 include:
[0015] Calcine manganese carbonate in air atmosphere at 600-900°C for 6-8h to obtain manganese trioxide;
[0016] After the manganese trioxide and the lithium hydroxide monohydrate are stirred and mixed, the transition metal is added, and a hydrothermal reaction is carried out at 210-270° C. for 10-12 hours, followed by centrifugation, washing with water, and drying to obtain an intermediate product;
[0017] The intermediate product was heated in air at 5 °C min -1 The temperature is raised to 400-600℃ at a heating rate for solid phase reaction for 3-5h to obtain the ion sieve precursor Li 1.6 (Mn M) 1.6 O4.
[0018] Optionally, the lithium hydroxide monohydrate and the manganese trioxide are stirred and mixed at a lithium to manganese molar ratio of 2:1.
[0019] Optionally, the step of subjecting the ion sieve precursor to acidification treatment comprises: adding the ion sieve precursor to a hydrochloric acid solution at 30-35° C. and stirring at a stirring speed of 380-420 r / min and a stirring time of 10-12 h.
[0020] Optionally, the first cross-linking agent is a mixture of one or more of hydroquinone, resorcinol and catechol.
[0021] Optionally, the second cross-linking agent is one of p-phenylenediamine and o-phenylenediamine, or a mixture of both.
[0022] Optionally, the multi-polymer is obtained by terpolymerization of acrylamide, 2-acrylamide-2-methylpropanesulfonic acid and vinyl pyrrolidone monomers.
[0023] Optionally, before drying the composite hydrogel, the method further comprises: washing the composite hydrogel with anhydrous ethanol and deionized water in sequence.
[0024] This application is based on the ion sieve precursor Li 1.6 Mn 1.6 O4 has poor structural stability, low ion sieve adsorption capacity, and is unstable in salt lake brine, underground brine, or gas field water. Transition metals are doped into the ion sieve precursor Li by hydrothermal reaction. 1.6 Mn 1.6 O4, an ion sieve H doped with a small amount of transition metal elements was prepared 1.6 (Mn M) 1.6 O4, which still maintains the spinel crystal structure. Ion sieve precursor Li 1.6 Mn 1.6 Mn in O4 3+ Due to its special 3d orbital electronic configuration (t 2g 3 -e g 1 ), will cause the Jahn-Teller effect, that is, the asymmetric occupation of electrons in degenerate orbits will cause the geometric configuration of the molecule to be distorted, thereby reducing the symmetry of the molecule and the degeneracy of the orbits, further reducing the energy of the system, and thus causing severe distortion of the octahedral lattice. This distortion will cause lithium ion sieving in Li + The stability and lithium extraction efficiency during the extraction / insertion process are reduced. Therefore, the present invention partially replaces Mn with transition metal elements. 3+ The position of Mn increases the degree of lattice disorder. 3+ The content of manganese is reduced, thereby increasing the total valence of manganese, inhibiting the Jahn-Teller effect, and thus increasing Li + The structural stability during embedding / extraction, and the numerous interfering ions such as Na + , K + , Ca 2 + Mg 2+ In the presence of + Still has good selectivity, thus improving the ion sieve H 1.6 (Mn M) 1.6 Adsorption capacity of O4.
[0025] In addition, the present application prepares a composite hydrogel containing an ion sieve. Since chitosan is unstable in salt lake brine, underground brine or gas field water with a high mineralization, a multi-polymer and a cross-linking system are used for cross-linking to increase the stability of the composite hydrogel. The multi-polymer introduces 2-acrylamide-2-methylpropane sulfonic acid and a functional monomer vinyl pyrrolidone on the basis of acrylamide. 2-acrylamide-2-methylpropane sulfonic acid has a hydrophilic sulfonic acid group. The introduction of the sulfonic acid group copolymer can improve the rigidity of the polymer molecule main chain, and 2-acrylamide-2-methylpropane sulfonic acid is relatively stable in a saline solution, thereby improving the salt resistance and hydrophilicity of the polymer, making it difficult to decompose in salt lake brine, underground brine or gas field water with a high mineralization. The vinyl pyrrolidone monomer has a cyclic structure and has a strong complexing ability. , the introduction of polymer molecular side chains can further improve the polymer stability and enhance the flocculation and coagulation of the hydrogel, and the first crosslinker and the second crosslinker will undergo a condensation reaction to generate a phenolic crosslinker, which can improve the reactivity of the crosslinking system, and the hydroxymethyl (-CH2OH) of the crosslinking system will undergo a condensation reaction with the main active group amide group (-CONH2) of the copolymer, which can make the linear copolymer form a three-dimensional network structure, and the benzene ring can be embedded when the copolymer and the phenolic crosslinker undergo a crosslinking reaction, thereby further improving the stability and tolerance of the composite hydrogel. Therefore, the composite hydrogel containing lithium ion sieve prepared in this application has good stability, is not easy to decompose in highly mineralized salt lake brine or underground brine or gas field water, and is resistant to Li + It has good adsorption properties, which solves the problem of low permeability of powdered ion sieves and difficulty in direct application. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0027] Spinel structure lithium manganese oxide Li 1.6 Mn 1.6 O4-based lithium ion sieve has become one of the most promising adsorbent materials for lithium extraction from salt lakes due to its high adsorption capacity and excellent lithium ion selectivity. However, the stable synthesis of ion sieve precursors is difficult, the adsorption capacity needs to be further improved, the structural stability is poor, and the ion sieve adsorbent powder material is difficult to apply directly. It has poor stability in highly mineralized salt lake brine, underground brine or gas field water, and the adsorption rate and adsorption capacity need to be further improved, which limits the industrial application of this type of adsorbent.
[0028] In view of the technical problems existing in the above-mentioned existing method for preparing lithium ion sieve adsorbent, an embodiment of the present application provides a method for preparing lithium ion sieve adsorbent, comprising the following steps:
[0029] The ion sieve precursor Li is prepared by using lithium-containing compounds and manganese salts as raw materials and doping with transition metal M by hydrothermal reaction. 1.6 (Mn M) 1.6 O4;
[0030] The above ion sieve precursor is subjected to acidification treatment to obtain ion sieve H 1.6 (Mn M) 1.6 O4;
[0031] Add the first crosslinking agent and the second crosslinking agent into water, heat and stir evenly to obtain a crosslinking system;
[0032] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0033] Adding a multi-component copolymer to the cross-linking system, adding the cross-linked copolymer to the chitosan solution, and then adding the ion sieve, stirring and mixing to obtain a composite hydrogel;
[0034] After the composite hydrogel is dried, an adsorbent containing a lithium ion sieve is obtained.
[0035] This application is based on the ion sieve precursor Li 1.6 Mn 1.6 O4 has poor structural stability and low adsorption capacity. Transition metals are doped into the ion sieve precursor Li by hydrothermal reaction. 1.6 Mn 1.6 O4, an ion sieve H doped with a small amount of transition metal elements was prepared 1.6 (Mn M) 1.6 O4, which still maintains the spinel crystal structure. Ion sieve precursor Li 1.6 Mn 1.6 Mn in O4 3 + Due to its special 3d orbital electronic configuration (t 2g 3 -e g 1 ), will cause the Jahn-Teller effect, that is, the asymmetric occupation of electrons in degenerate orbits will cause the geometric configuration of the molecule to be distorted, thereby reducing the symmetry of the molecule and the degeneracy of the orbits, further reducing the energy of the system, and thus causing severe distortion of the octahedral lattice. This distortion will cause lithium ion sieving in Li + The stability and lithium extraction efficiency during the extraction / insertion process are reduced. Therefore, the present invention partially replaces Mn with transition metal elements. 3+The position of Mn increases the degree of lattice disorder. 3+ The content of manganese is reduced, thereby increasing the total valence of manganese, inhibiting the Jahn-Teller effect, and thus increasing Li + The structural stability during embedding / extraction, and the numerous interfering ions such as Na + , K + , Ca 2+ Mg 2+ In the presence of + Still has good selectivity, thus improving the ion sieve H 1.6 (Mn M) 1.6 Adsorption capacity of O4.
[0036] In addition, the present application prepares the composite hydrogel containing ion sieves. Since chitosan is unstable in highly mineralized salt lake brine, underground brine or gas field water, a multi-polymer and a cross-linking system are used for cross-linking to increase the stability of the composite hydrogel. Therefore, the composite hydrogel containing lithium ion sieves prepared in the present application has good stability and is not easy to decompose in highly mineralized salt lake brine, underground brine or gas field water. + It has good adsorption properties, which solves the problem of low permeability of powdered ion sieves and difficulty in direct application.
[0037] Specifically, when the composite hydrogel containing ion sieve prepared in the present application is applied to carbonate salt lake brine, since the pH value of carbonate salt lake brine is between 8 and 11, there are more OH - , which can neutralize the lithium ion sieve in the adsorption of Li + The H released + , so that the competing ion H + The competitiveness of the hydrogel is weakened, which promotes the reaction to the right and increases the adsorption capacity. At the same time, the surface potential of the hydrogel gradually decreases with the increase of pH value, and more negative charges exist on the surface of the lithium ion sieve, thereby + It has a greater affinity, which is beneficial for lithium ion sieve to Li + adsorption.
[0038] As an implementation method of the present application, the lithium-containing compound is lithium hydroxide monohydrate LiOH·H2O; and the manganese salt is manganese carbonate MnCO3.
[0039] As an embodiment of the present application, the above transition metal includes cobalt and copper. Cobalt and copper are doped into the ion sieve precursor Li 1.6 Mn 1.6 O4, prepare Li 1.6 (Mn M) 1.6O4, the obtained ion sieve precursor has higher structural stability and also has good stability during the cyclic adsorption process.
[0040] As an implementation method of the present application, the above-mentioned hydrothermal reaction method is used to prepare the ion sieve precursor Li 1.6 (MnM) 1.6 The steps of O4 include:
[0041] Calcine manganese carbonate in air atmosphere at 600-900°C for 6-8h to obtain manganese trioxide;
[0042] After the manganese trioxide and the lithium hydroxide monohydrate are stirred and mixed, the transition metal is added, and a hydrothermal reaction is carried out at 210-270° C. for 10-12 hours, followed by centrifugation, washing with water, and drying to obtain an intermediate product;
[0043] The intermediate product was heated in air at 5 °C min -1 The temperature is raised to 400-600℃ at a heating rate for solid phase reaction for 3-5h to obtain the ion sieve precursor Li 1.6 (Mn M) 1.6 O4.
[0044] As an implementation method of the present application, the lithium hydroxide monohydrate and the manganese trioxide are stirred and mixed at a lithium-manganese molar ratio of 2:1.
[0045] As an implementation method of the present application, the above-mentioned ion sieve precursor is subjected to an acidification treatment step, comprising: adding the above-mentioned ion sieve precursor to a hydrochloric acid solution at 30-35°C and stirring, with a stirring speed of 380-420r / min and a stirring time of 10-12h. During the acidification treatment, the extraction / embedding of lithium ions does not belong to the redox mechanism, but is carried out according to the ion exchange mechanism between lithium ions and hydrogen ions, which is expressed as follows:
[0046] Li 1.6 (Mn M) 1.6 O4+HCl→H 1.6 (Mn M) 1.6 O4+LiCl
[0047] As an implementation method of the present application, the first crosslinking agent is a mixture of one or more of hydroquinone, resorcinol and catechol. Hydroquinone, resorcinol and catechol all contain phenolic hydroxyl groups, which can undergo condensation reaction with the main active group amide group of the copolymer, and embed the benzene ring during crosslinking, so that the linear copolymer forms a three-dimensional network structure, thereby improving the flocculation effect of the hydrogel.
[0048] As an implementation method of the present application, the second crosslinking agent is one or a mixture of p-phenylenediamine and o-phenylenediamine. p-phenylenediamine and o-phenylenediamine contain benzene rings and amino groups (-NH), which can undergo condensation reaction with the amide group, the main active group of the multi-polymer, and embed the benzene ring during crosslinking, thereby improving the stability of the hydrophilic chitosan.
[0049] As an implementation method of the present application, the above-mentioned multi-polymer is obtained by ternary copolymerization of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and vinyl pyrrolidone monomers. On the basis of acrylamide, the multi-polymer further introduces 2-acrylamide-2-methylpropane sulfonic acid and functional monomer vinyl pyrrolidone. 2-acrylamide-2-methylpropane sulfonic acid has a hydrophilic sulfonic acid group. The introduction of the sulfonic acid group copolymerization can improve the rigidity of the polymer molecule main chain, and 2-acrylamide-2-methylpropane sulfonic acid is relatively stable in a saline solution, thereby improving the salt resistance and hydrophilicity of the polymer, making it difficult to decompose in highly mineralized salt lake brine or underground brine or gas field water. The vinyl pyrrolidone monomer has a cyclic structure and has a strong complexing ability. The introduction of the polymer molecule side chain can further improve the polymer stability, enhance the flocculation and coagulation of the hydrogel, solve the problem of poor stability of the chitosan solution, and further improve the stability and tolerance of the composite hydrogel.
[0050] As an implementation method of the present application, before drying the composite hydrogel, the method further includes: washing the composite hydrogel with anhydrous ethanol and deionized water in sequence.
[0051] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.
[0052] Example 1
[0053] A method for preparing a lithium ion sieve adsorbent comprises the following steps:
[0054] MnCO3 was calcined at 750°C in air atmosphere for 7 h to obtain Mn2O3;
[0055] LiOH·H2O and the above-mentioned Mn2O3 were stirred and mixed at a lithium-manganese ratio of 4:1, and then transition metal Co was added to carry out a hydrothermal reaction at 240°C for 11 hours. After centrifugation, washing with water, and drying, an intermediate product was obtained;
[0056] The intermediate product was heated in air at 5 °C min -1 The temperature was raised to 500 °C at a heating rate of 4 h to obtain the ion sieve precursor Li 1.6 (Mn Co) 1.6 O4;
[0057] The above ion sieve precursor was added into the hydrochloric acid solution and stirred at 32°C at a speed of 400 r / min for 11 h to obtain the ion sieve H 1.6 (Mn Co) 1.6 O4;
[0058] Adding a first crosslinking agent and a second crosslinking agent into water, heating and stirring uniformly to obtain a crosslinking system, wherein the first crosslinking agent is a mixture of hydroquinone, resorcinol and catechol, and the second crosslinking agent is a mixture of p-phenylenediamine and o-phenylenediamine;
[0059] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0060] Adding a multi-polymer to the cross-linking system, adding it to the chitosan solution after cross-linking, and then adding the ion sieve, stirring and mixing to obtain a composite hydrogel, wherein the multi-polymer is obtained by ternary copolymerization of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and vinyl pyrrolidone monomers;
[0061] The composite hydrogel is washed with anhydrous ethanol and deionized water in turn, and then dried to obtain an adsorbent containing a lithium ion sieve.
[0062] Example 2
[0063] A method for preparing a lithium ion sieve adsorbent comprises the following steps:
[0064] MnCO3 was calcined at 600°C in air atmosphere for 8 h to obtain Mn2O3;
[0065] LiOH·H2O and the above-mentioned Mn2O3 were stirred and mixed at a lithium-manganese ratio of 4:1, and then transition metal Cu was added to carry out a hydrothermal reaction at 210°C for 12 hours. After centrifugation, washing with water, and drying, an intermediate product was obtained;
[0066] The intermediate product was heated in air at 5 °C min -1 The temperature was raised to 400 °C at a heating rate of 1.5 °C for solid phase reaction for 3 h to obtain the ion sieve precursor Li 1.6 (MnCu) 1.6 O4;
[0067] The above ion sieve precursor was added into the hydrochloric acid solution at 30°C and stirred at a speed of 380 r / min for 12 h to obtain the ion sieve H 1.6 (MnCu) 1.6 O4;
[0068] Add a first crosslinking agent and a second crosslinking agent into water, heat and stir evenly to obtain a crosslinking system, wherein the first crosslinking agent is hydroquinone and the second crosslinking agent is o-phenylenediamine;
[0069] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0070] Adding a multi-polymer to the cross-linking system, adding it to the chitosan solution after cross-linking, and then adding the ion sieve, stirring and mixing to obtain a composite hydrogel, wherein the multi-polymer is obtained by ternary copolymerization of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and vinyl pyrrolidone monomers;
[0071] The composite hydrogel is washed with anhydrous ethanol and deionized water in turn, and then dried to obtain an adsorbent containing a lithium ion sieve.
[0072] Example 3
[0073] A method for preparing a lithium ion sieve adsorbent comprises the following steps:
[0074] MnCO3 was calcined at 900℃ in air atmosphere for 6h to obtain Mn2O3;
[0075] LiOH·H2O and the above-mentioned Mn2O3 were stirred and mixed at a lithium-manganese ratio of 4:1, and then transition metal Co was added to carry out a hydrothermal reaction at 270°C for 10 hours. After centrifugation, washing with water, and drying, an intermediate product was obtained;
[0076] The intermediate product was heated in air at 5 °C min -1 The temperature was raised to 600 °C at a heating rate of 500 °C for solid phase reaction. The reaction time was 5 h to obtain the ion sieve precursor Li 1.6 (Mn Co) 1.6 O4;
[0077] The above ion sieve precursor was added into the hydrochloric acid solution and stirred at 35°C at a speed of 420 r / min for 10 h to obtain the ion sieve H 1.6 (Mn Co) 1.6 O4;
[0078] Adding a first crosslinking agent and a second crosslinking agent into water, heating and stirring uniformly to obtain a crosslinking system, wherein the first crosslinking agent is a mixture of resorcinol and catechol, and the second crosslinking agent is p-phenylenediamine;
[0079] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0080] Adding a multi-polymer to the cross-linking system, adding it to the chitosan solution after cross-linking, and then adding the ion sieve, stirring and mixing to obtain a composite hydrogel, wherein the multi-polymer is obtained by ternary copolymerization of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and vinyl pyrrolidone monomers;
[0081] The composite hydrogel is washed with anhydrous ethanol and deionized water in turn, and then dried to obtain an adsorbent containing a lithium ion sieve.
[0082] Comparative Example 1
[0083] Compared with Example 1, the ion sieve precursor Li 1.6 (Mn Co) 1.6 When O4 is used, no transition metal is doped and the rest of the steps are the same.
[0084] Comparative Example 2
[0085] Ion sieve H was prepared according to the steps of Example 1 1.6 (Mn Co) 1.6 O4;
[0086] Adding a first crosslinking agent and a second crosslinking agent into water, heating and stirring uniformly to obtain a crosslinking system, wherein the first crosslinking agent is a mixture of hydroquinone, resorcinol and catechol, and the second crosslinking agent is a mixture of p-phenylenediamine and o-phenylenediamine;
[0087] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0088] Adding the cross-linking system to the chitosan solution, and then adding the ion sieve, stirring and mixing, to obtain a composite hydrogel;
[0089] The composite hydrogel is washed with anhydrous ethanol and deionized water in turn, and then dried to obtain an adsorbent containing a lithium ion sieve.
[0090] Comparative Example 3
[0091] Prepare ion sieve H according to the steps of Example 1 1.6 (Mn Co) 1.6 O4;
[0092] dissolving chitosan in acetic acid solution to obtain a chitosan solution;
[0093] Adding a multi-component copolymer to the chitosan solution, and then adding the ion sieve, stirring and mixing, to obtain a composite hydrogel, wherein the multi-component copolymer is obtained by ternary copolymerization of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and vinyl pyrrolidone monomers;
[0094] The composite hydrogel is washed with anhydrous ethanol and deionized water in turn, and then dried to obtain an adsorbent containing a lithium ion sieve.
[0095] Experimental example
[0096] (I) Detection of ion sieve precursor Li 1.6 (Mn M) 1.6 Stability of O4
[0097] Weigh 1g of the ion sieve precursor prepared in Examples 1-3 and Comparative Example 1 of the present application, add it to a conical flask containing 100ml of deionized water, seal it, put it into an ultrasonic oscillator at room temperature, shake it for 24h, then filter it, dry it at 50°C for 24h, weigh the mass of the ion sieve precursor after drying, and calculate its mass loss rate according to formula (1). The greater the mass loss, the worse the stability of the ion sieve precursor. The test results are shown in Table 1 below.
[0098] w=(m0-m e ) / m0×100% (1)
[0099] Where: w is the mass loss rate of the sample, %; m0 is the mass of the added sample, g; m e is the mass of the sample after treatment, g.
[0100] Table 1
[0101] Group Example 1 Example 2 Example 3 Comparative Example 1 W(%) 0.07 0.08 0.07 0.14
[0102] As shown in Table 1, the ion sieve precursor prepared in the embodiment of the present application has good stability, while in Comparative Example 1, due to the absence of transition metal doping, the spinel crystal structure is easily distorted. + Poor structural stability during insertion / removal.
[0103] (II) Determination of the adsorption selectivity of the ion sieve adsorbent of the present application for lithium ions
[0104] The pH of the salt lake brine was adjusted to 10 with ammonia-ammonium chloride buffer solution (molar ratio 4:1), and the ion sieve adsorbents prepared in Examples 1-3 and Comparative Examples 1-3 of the present application were added in groups at a solid-liquid ratio of 1 g / L at 35°C, and adsorbed with magnetic stirring for 24 hours. Samples were taken and the contents of various ions were determined by ICP (inductively coupled plasma atomic emission spectroscopy). The selective adsorption performance can be measured by the distribution coefficient K D and separation coefficient α(Li / Me), K D is the distribution coefficient of metal ions in salt lake brine solution. α(Li / Me) is used to analyze Li + The separation degree from other metal ions is shown in equations (2) and (3). The test results are shown in Table 2 below.
[0105] K D =q e / ρ e (2)
[0106] α(Li / Me)=K D1 / K D2 (3)
[0107] Where: q e is the equilibrium adsorption capacity, mg / g; ρ e is the equilibrium mass concentration, mg / L; K D1 For Li + Distribution coefficient of adsorption, mL / g; K D2 For other metal ions (K + , Ca 2+ 、Na + Mg 2+ ) Partition coefficient of adsorption, mL / g.
[0108] ρ0 is the initial mass concentration.
[0109] Table 2
[0110] ion <![CDATA[ρ0(mg / L)]]> <![CDATA[ρ e (mg / L)]]> <![CDATA[q e (mg / g)]]> <![CDATA[K D (mL / g)]]> α(Li / Me) <![CDATA[Li + ]]> 201.32 178.85 22.47 125.63 1.00 <![CDATA[K + ]]> 79.47 78.58 0.89 11.33 11.09 <![CDATA[Ca 2+ ]]> 102.64 101.21 1.43 14.13 8.89 <![CDATA[Na + ]]> 179.47 179.11 0.36 2.01 62.50 <![CDATA[Mg 2+ ]]> 386.79 384.82 1.97 5.12 24.54
[0111] As can be seen from Table 2, the lithium ion sieve adsorbent prepared in the embodiment of the present application has a much greater adsorption selectivity for lithium ions than the adsorbent prepared in the comparative example. Since no transition metal is doped in comparative example 1, no multipolymer is added in comparative example 2, and no cross-linking agent is added for cross-linking in comparative example 3, the stability of the adsorbent and the lithium extraction efficiency are affected. This shows that the lithium ion sieve adsorbent prepared in the embodiment of the present application has good selectivity for lithium ions and can improve the adsorption capacity of lithium.
[0112] The above description is only an optional embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural transformations made using the contents of the present application specification under the inventive concept of the present application, or direct / indirect application in other related technical fields are included in the patent protection scope of the present application.
Claims
1. A method for preparing a lithium ion sieve adsorbent, characterized in that: The following steps are involved: The ion sieve precursor Li is prepared by using lithium-containing compounds and manganese salts as raw materials and doping with transition metal M by hydrothermal reaction. 1.6 (Mn M) 1.6 O4; The ion sieve precursor is subjected to acidification treatment to obtain ion sieve H 1.6 (Mn M) 1.6 O4; Add a first crosslinking agent and a second crosslinking agent into water, heat and stir evenly to obtain a crosslinking system; wherein the first crosslinking agent is a mixture of one or more of hydroquinone, resorcinol and catechol; and the second crosslinking agent is a mixture of one or two of p-phenylenediamine and o-phenylenediamine; dissolving chitosan in acetic acid solution to obtain a chitosan solution; Adding a multi-component copolymer to the cross-linking system, adding it to the chitosan solution after cross-linking, and then adding the ion sieve, stirring and mixing to obtain a composite hydrogel; wherein the multi-component copolymer is obtained by ternary copolymerization of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and vinyl pyrrolidone monomers; After the composite hydrogel is dried, an adsorbent containing a lithium ion sieve is obtained.
2. The method for preparing the lithium ion sieve adsorbent according to claim 1, characterized in that: The lithium-containing compound is lithium hydroxide monohydrate; and the manganese salt is manganese carbonate.
3. The method for preparing the lithium ion sieve adsorbent according to claim 2, characterized in that: The transition metals include cobalt and copper.
4. The method for preparing the lithium ion sieve adsorbent according to claim 3, characterized in that: The hydrothermal reaction method is used to prepare the ion sieve precursor Li 1.6 (Mn M) 1.6 The steps of O4 include: Calcine manganese carbonate in air atmosphere at 600-900°C for 6-8h to obtain manganese trioxide; After the manganese trioxide and the lithium hydroxide monohydrate are stirred and mixed, the transition metal is added, and a hydrothermal reaction is carried out at 210-270° C. for 10-12 hours, followed by centrifugation, washing with water, and drying to obtain an intermediate product; The intermediate product was heated in air at 5 °C·min -1 The temperature is raised to 400-600℃ at a heating rate for solid phase reaction for 3-5h to obtain the ion sieve precursor Li 1.6 (Mn M) 1.6 O4.
5. The method for preparing the lithium ion sieve adsorbent according to claim 4, characterized in that: The lithium hydroxide monohydrate and the manganese trioxide are stirred and mixed at a lithium-manganese molar ratio of 2:
1.
6. The method for preparing a lithium ion sieve adsorbent according to claim 1, characterized in that: The step of subjecting the ion sieve precursor to acidification treatment comprises: adding the ion sieve precursor into a hydrochloric acid solution at 30-35° C. and stirring at a stirring speed of 380-420 r / min and a stirring time of 10-12 h.
7. The method for preparing a lithium ion sieve adsorbent according to claim 1, characterized in that: Before drying the composite hydrogel, the method further comprises: washing the composite hydrogel with anhydrous ethanol and deionized water in sequence.