A carbon-based composite material and its preparation method and application
The biomineralization method enriches metal ions in carbon materials and forms catalysts, which solves the problems of high nucleation overvoltage and low Coulombic efficiency of traditional carbon materials in alkali metal negative electrodes, and improves the electrochemical performance and cycle life of the battery.
Patent Information
- Application Number
- CN202410254371.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-06
AI Technical Summary
Traditional carbon materials have problems such as high nucleation overvoltage, low Coulombic efficiency, and poor cycle performance in alkali metal anodes. This is mainly due to the single pore structure, low specific surface area, and low alkali metal affinity, which leads to the current density distribution of the battery during the charge and discharge process. Unevenness and volume expansion affect the rate performance and cycle life of the battery.
The biomineralization method is used to enrich metal ions in biomass to form a catalyst, and carbon tubes are grown on the surface of the carbon material through pyrolysis and carbonization processes to increase the specific surface area and conductivity, thereby improving electrochemical performance.
The nucleation overvoltage is reduced, the Coulombic efficiency and cycle life are improved, the electrochemical performance of the alkali metal anode is improved, and better battery rate performance and stability are achieved.
Smart Images

Figure CN118005002B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery negative electrode materials, and in particular to a carbon-based composite material and a preparation method and application thereof. Background Art
[0002] Carbon materials have excellent conductivity, wide sources, good elastic modulus, and carbon materials with three-dimensional spatial structures do not require binders and conductive additives when used as hosts, thereby reducing costs and increasing energy density. At the same time, because carbon materials are easy to control the pore structure and have a large specific surface area, carbon materials can have more space for storage to alleviate volume expansion. These advantages make carbon materials competent as alkali metal negative electrode hosts.
[0003] In 2021, Kim et al. constructed a defect-rich carbon current collector and combined it with LixNi 0.8 Co 0.1 Mn 0.1 The battery is a full battery with a base cathode and a non-aqueous lithium-containing electrolyte solution. Under low electrolyte conditions, these batteries maintain 90% of their initial capacity for more than 50 cycles. At present, the academic community has accelerated the reaction kinetics by introducing metals and their metal compounds into the host material to increase its sodium affinity. In 2022, Lee et al. used three-dimensional nanostructured porous carbon particles containing carbon shells coated with iron nanoparticles as highly reversible sodium metal hosts. In a half-cell, at 10 mA cm -2 and 10 mAh cm -2 Under these conditions, high reversibility was achieved over 500 cycles with a Coulombic efficiency of 99.6% at 60 mA cm -2 Under the same conditions, more than 14,400 cycles were achieved in a symmetric battery. In 2022, Gong et al. constructed copper sulfide nanosheets for lithium metal anode and achieved a charge transfer rate of 1 mA cm -2 Ultra-smooth and dense lithium deposition is possible at 10 mAh cm -2 The average thickness under the conditions is ≈53.0 μm, which is close to the theoretical lithium foil thickness and is highly reversible under different cycles.
[0004] However, the idea of introducing metals and their metal compounds on carbon materials makes the preparation process cumbersome, and the catalyst loading of the resulting host material is often low, making it difficult to achieve the purpose of improving the electrochemical performance of the host material. Biomineralization, as a common phenomenon in nature, refers to the process by which organic life regulates the formation of inorganic minerals. In a suitable environment, organic macromolecules in cells adsorb nearby positively charged inorganic metal ions through electrostatic action, especially biomacromolecules rich in carboxyl, hydroxyl and amino groups at the end of the molecular chain. In addition, there are some special proteins on the surface of biological cells that can recognize and bind to some special metal ions. For example, nerve cells in the human brain achieve the balance of sodium and potassium ions inside and outside the cell through special proteins on the surface of the cell membrane to achieve the transmission of electrical signals. After enriching inorganic metal ions, organisms accurately assemble into the required inorganic compounds under the action of enzymes. Because of the above advantages, biomineralization can easily achieve self-assembly at the nanoscale, thereby greatly reducing the synthesis steps of materials, and the metal ions are evenly distributed due to the action of physical bonds or chemical bonds. At present, the synthesis method of biomineralization is common in environmental governance and medicine, but rarely in the energy field. By utilizing the biomineralization method of biomass (including bamboo, basswood, mushroom residue, etc.) to synthesize catalysts for use in alkali metal negative electrodes, it is possible to effectively solve the disadvantages of high cost and poor battery performance caused by the cumbersome traditional preparation methods and limited effects.
[0005] Alkali metal anodes have been widely studied due to their excellent specific capacity. However, due to the single pore structure, low specific surface area and low affinity for alkali metals, traditional current collectors have too high nucleation overvoltage during the charge and discharge process, resulting in higher voltage hysteresis, and the battery exhibits poor rate performance. At the same time, traditional current collectors are prone to uneven current density distribution under high current density charge and discharge conditions, and because of their limited storage volume, they lead to the generation of inactive substances, dendrite growth, volume expansion, and reduced coulombic efficiency, resulting in poor battery cycle performance. Summary of the invention
[0006] The purpose of the present invention is to provide a carbon-based composite material and a preparation method and application thereof, and to provide a carbon material loaded with a catalyst obtained by a biomineralization method, wherein biomass is used as a carbon source and its biomineralization effect is utilized to allow metal ions to spontaneously and uniformly accumulate inside the biomass and form a catalyst; carbon tubes are grown on the surface of the carbon material using the catalyst generated by the metal ions enriched inside the biomass, thereby increasing the specific surface area and conductivity of the carbon material and improving its electrochemical performance.
[0007] To achieve the above object, the present invention provides a method for preparing a carbon-based composite material, comprising the following steps:
[0008] S1. Dissolve the metal salt in deionized water, and stir with a magnetic stirrer until the metal salt is completely dissolved to obtain a metal salt solution;
[0009] S2, immersing the biomass in a metal salt solution, utilizing the mineralization of the biomass to enrich the metal salt and realize self-assembly to obtain a precursor;
[0010] S3, freeze-drying the precursor obtained in step S2 to obtain a sample;
[0011] S4, pyrolyzing and carbonizing the sample in an argon atmosphere to obtain a carbon-metal composite material;
[0012] S5, placing the carbon-metal composite material obtained in step S4 in an acidic solution to soak and remove excess metal particles, then washing with deionized water until neutral and placing in an oven for heat preservation to obtain carbonized biomass;
[0013] S6, the biomass carbonized in step S5 is passed through sandpaper and a punch to obtain a carbon sheet;
[0014] S7, further subjecting the carbon sheet obtained in step S6 to high-temperature carbonization, and placing melamine upstream thereof to generate a carbon-based composite material.
[0015] Preferably, in step S1, the metal salt is any one of iron salt, cobalt salt and nickel salt; the mass ratio of metal salt to deionized water is 40-162:10000; the stirring temperature is 25°C; the stirring rate is 200-600r / min; and the concentration of the metal salt solution is 0.05-0.2mol / L.
[0016] Preferably, in step S2, the biomass is agricultural waste such as mushroom residue, basswood, bamboo, etc.; the mass ratio of the biomass to the metal salt solution is 4 to 8:100; and the immersion time is 10 to 48 hours.
[0017] Preferably, in step S3, freeze drying is performed by keeping warm in an environment of -50°C for 1 to 5 hours, and then drying in an environment of 20°C for 24 to 48 hours.
[0018] Preferably, in step S4, the carbonization temperature is 800-1000° C. and the carbonization time is 60 min.
[0019] Preferably, in step S5, the acid solution is a hydrochloric acid solution with a concentration of 1 to 2 mol / L; the soaking time is 5 to 10 hours; the insulation time is 10 to 24 hours; and the insulation temperature is 50 to 80°C.
[0020] Preferably, in step S6, the carbon sheet has a thickness of 0.55 to 0.65 mm and a diameter of 8 to 10 mm.
[0021] Preferably, in step S7, the high temperature carbonization process is firstly to increase the temperature to 180°C at 5°C / min and keep the temperature for 2h, and then to increase the temperature to 680°C at 2°C / min and keep the temperature for 4h;
[0022] The mass ratio of the carbon sheet to melamine is 1:240-400.
[0023] The invention also provides a carbon-based composite material prepared by a method for preparing the carbon-based composite material.
[0024] The present invention also provides an application of a carbon-based composite material in an alkali metal negative electrode carrier.
[0025] Therefore, the present invention adopts the above-mentioned carbon-based composite material and its preparation method and application, and its technical effects are as follows:
[0026] (1) A method for obtaining a carbon material loaded with a catalyst using biomineralization is provided, wherein biomass is used as a carbon source and the biomineralization effect thereof is utilized to allow metal ions to spontaneously and uniformly accumulate inside the biomass and form a catalyst.
[0027] (2) Using the catalyst generated by the metal ions enriched in the biomass to grow carbon nanotubes on the surface of the carbon material, thereby increasing the specific surface area and conductivity of the carbon material and improving its electrochemical performance.
[0028] (3) Provide a carbon material for alkali metal negative electrode, which is prepared by the above method and has simple preparation, low cost and excellent electrochemical performance. When used as an alkali metal negative electrode, it can reduce the nucleation overvoltage, improve the coulombic efficiency, increase the cycle life and rate performance.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the XRD diagram of Example 1 of the present invention;
[0031] Figure 2 This is a rate diagram of a sodium metal negative electrode symmetric battery according to Example 1 of the present invention.
[0032] Figure 3 This is a long cycle diagram of the sodium metal negative electrode symmetric battery of Example 1 of the present invention
[0033] Figure 4 The coulombic efficiency and cycle number of the sodium metal negative electrode half-cell of the first embodiment of the present invention are shown in FIG. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0035] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0036] Embodiment 1
[0037] Step 1: Dissolve 0.81 g of ferric chloride in 50 mL of deionized water, and stir with a magnetic stirrer at room temperature and at a speed of 200 r / min until the ferric chloride is completely dissolved.
[0038] Step 2: Wash the dried mushroom roots with deionized water and soak them for 5 hours. After soaking, take them out, cut them into 0.5 cm thick slices, and place them in an oven at 60°C for drying.
[0039] Step 3: Soak the mushroom slices in step 2 in the ferric chloride solution in step 1 for 24 hours.
[0040] Step 4: Take out the mushroom slices in step 3 and place them in a cold trap for freezing for 5 hours, and then dry them for 24 to 48 hours.
[0041] Step 5: The sample in step 4 was heated to 1000°C at a heating rate of 5°C / min using a tube furnace under argon conditions and maintained at 1000°C for 1 hour.
[0042] Step 6: Place the carbon material after pyrolysis in step 5 into 1 mol / L hydrochloric acid and let it stand for 5 hours, wash it with deionized water to neutralize it and place it in a 60°C oven for 12 hours.
[0043] Step 7: The mushroom slices carbonized in step 6 are passed through sandpaper and punches to obtain cylindrical carbon sheets with a thickness of 0.55 mm to 0.65 mm and a diameter of 8 to 10 mm.
[0044] Step 8: The carbon sheet prepared in step 7 is further carbonized at high temperature, and 1.2 g of melamine is placed upstream of the carbon sheet;
[0045] The heating curve is as follows: first increase the temperature to 180°C at 5°C / min and keep it for 2h, then increase the temperature to 680°C at 2°C / min and keep it for 4h.
[0046] Embodiment 2
[0047] Step 1: Dissolve 0.81 g of ferric chloride in 50 mL of deionized water, and stir with a magnetic stirrer at room temperature and at a speed of 200 r / min until the ferric chloride is completely dissolved.
[0048] Step 2: Wash the dried mushroom roots with deionized water and soak them for 5 hours. After soaking, take them out, cut them into 0.5 cm thick slices, and place them in an oven at 60°C for drying.
[0049] Step 3: Soak the mushroom slices in step 2 in the ferric chloride solution in step 1 for 24 hours.
[0050] Step 4: Take out the mushroom slices in step 3 and place them in a cold trap for freezing for 5 hours, and then dry them for 24 to 48 hours.
[0051] Step 5: The sample prepared in step 4 was heated to 900°C at a heating rate of 5°C / min in a tube furnace under argon gas and maintained at 900°C for 1 hour.
[0052] Step 6: Place the carbon material after pyrolysis in step 5 into 1 mol / L hydrochloric acid and let it stand for 5 hours, wash it with deionized water to neutralize it and place it in a 60°C oven for 12 hours.
[0053] Step 7: The mushroom slices carbonized in step 6 are passed through sandpaper and punches to obtain cylindrical carbon sheets with a thickness of 0.55 mm to 0.65 mm and a diameter of 8 to 10 mm.
[0054] Step 8: The carbon sheet prepared in step 7 is further carbonized at high temperature, and 1.2 g of melamine is placed upstream of the carbon sheet;
[0055] The heating curve is: first increase the temperature to 180℃ at 5℃ / min and keep it for 2h, then increase the temperature to 680℃ at 2℃ / min and keep it for 4h
[0056] Embodiment 3
[0057] Step 1: Dissolve 0.81 g of ferric chloride in 50 mL of deionized water, and stir with a magnetic stirrer at room temperature and at a speed of 200 r / min until the ferric chloride is completely dissolved.
[0058] Step 2: Wash the dried mushroom roots with deionized water and soak them for 5 hours. After soaking, take them out, cut them into 0.5 cm thick slices, and place them in an oven at 60°C for drying.
[0059] Step 3: Soak the mushroom slices in step 2 in the ferric chloride solution in step 1 for 24 hours.
[0060] Step 4: Take out the mushroom slices in step 3 and place them in a cold trap for freezing for 5 hours, and then dry them for 24 to 48 hours.
[0061] Step 5: The sample in step 4 was heated to 800°C at a heating rate of 5°C / min using a tube furnace under argon conditions and maintained at a constant temperature of 800°C for 1 hour.
[0062] Step 6: Place the carbon material after pyrolysis in step 5 into 1 mol / L hydrochloric acid and let it stand for 5 hours, wash it with deionized water to neutralize it and place it in a 60°C oven for 12 hours.
[0063] Step 7: The mushroom slices carbonized in step 6 are passed through sandpaper and punches to obtain cylindrical carbon sheets with a thickness of 0.55 mm to 0.65 mm and a diameter of 8 to 10 mm.
[0064] Step 8: The carbon sheet prepared in step 7 is further carbonized at high temperature, and 1.2 g of melamine is placed upstream of the carbon sheet;
[0065] The heating curve is: first increase to 180°C at 5°C / min and keep warm for 2h, then increase to 680°C at 2°C / min and keep warm for 4h.
[0066] Embodiment 4
[0067] Step 1: Dissolve 1.45 g of nickel nitrate in 50 mL of deionized water, and stir with a magnetic stirrer at room temperature and at a speed of 200 r / min until the ferric chloride is completely dissolved.
[0068] Step 2: Wash the dried mushroom roots with deionized water and soak them for 5 hours. After soaking, take them out, cut them into 0.5 cm thick slices, and place them in an oven at 60°C for drying.
[0069] Step 3: Soak the mushroom slices in step 2 in the nickel nitrate solution in step 1 for 24 hours.
[0070] Step 4: Take out the mushroom slices in step 3 and place them in a cold trap for freezing for 5 hours, and then dry them for 24 to 48 hours.
[0071] Step 5: The sample prepared in step 4 was heated to 1000°C at a heating rate of 5°C min-1 in a tube furnace under argon gas and maintained at 1000°C for 1 h.
[0072] Step 6: Place the carbon material after pyrolysis in step 5 into 1 mol / L hydrochloric acid and let it stand for 5 hours, wash it with deionized water to neutralize it and place it in a 60°C oven for 12 hours.
[0073] Step 7: The mushroom slices carbonized in step 6 are passed through sandpaper and punches to obtain cylindrical carbon sheets with a thickness of 0.55 mm to 0.65 mm and a diameter of 8 to 10 mm.
[0074] Step 8: The carbon sheet prepared in step 7 is further carbonized at high temperature, and 1.2 g of melamine is placed upstream of the carbon sheet;
[0075] The heating curve is: first increase the temperature to 180℃ at 5℃ / min and keep it for 2h, then increase the temperature to 680℃ at 2℃ / min and keep it for 4h
[0076] Comparative Example 1
[0077] Step 1: Wash the dried mushroom roots with deionized water and soak them for 5 hours. After soaking, take them out, cut them into 0.5 cm thick slices, and place them in an oven at 60°C for drying.
[0078] Step 2: Soak the mushroom slices in step 1 in deionized water for 24 hours.
[0079] Step 3: Take out the mushroom slices in step 2 and place them in a cold trap for freezing for 5 hours, and then dry them for 24 to 48 hours.
[0080] Step 4: Heat the sample prepared in step 3 to 1000°C at a heating rate of 5°C / min in a tube furnace under argon and maintain the temperature at 1000°C for 1 hour.
[0081] Step 5: Place the carbon material after pyrolysis in step 4 into 1 mol / L hydrochloric acid and let it stand for 5 hours, wash it with deionized water to neutralize it and place it in a 60°C oven for 12 hours.
[0082] Comparative Example 2
[0083] Step 1: Wash the dried mushroom roots with deionized water and soak them for 5 hours. After soaking, take them out, cut them into 0.5 cm thick slices, and place them in an oven at 60°C for drying.
[0084] Step 2: Soak the mushroom slices in step 1 in deionized water for 24 hours.
[0085] Step 3: Take out the mushroom slices in step 2 and place them in a cold trap for freezing for 5 hours, and then dry them for 24 to 48 hours.
[0086] Step 4: Heat the sample prepared in step 3 to 1000°C at a heating rate of 5°C / min in a tube furnace under argon and maintain the temperature at 1000°C for 1 hour.
[0087] Step 5: Place the carbon material after pyrolysis in step 4 into 1 mol / L hydrochloric acid and let it stand for 5 hours, wash it with deionized water to neutralize it and place it in a 60°C oven for 12 hours.
[0088] Table 1 The above samples match sodium at a current density of 1 mA cm -2 The first nucleation overvoltage and polarization voltage
[0089]
[0090]
[0091] As shown in Table 1, among various metal salts, iron salts have better nucleation overvoltage and polarization voltage than nickel salts, and have a higher affinity for metallic sodium. The former battery also shows better stability. Similarly, the sample calcined at 1000℃ has better performance.
[0092] like Figure 1As shown, the physical phase of Example 1 is mainly graphite carbon, and the ferric chloride is reduced to α-Fe and Fe3C after carbonization, so that the sodium affinity is enhanced.
[0093] like Figure 2 As shown, the sodium metal symmetric battery of Example 1 is -2 The current density below 10 mA cm -2 Cycling can also be achieved at high current density.
[0094] like Figure 3 As shown, the sodium metal symmetric battery of Example 1 is -2 The current density below is stable, and the polarization voltage is stable at about 80mV after nearly 1000h of cycling.
[0095] like Figure 4 As shown, the sodium metal half-cell of Example 1 is -2 The coulombic efficiency is stable at the following current densities.
[0096] Therefore, the present invention adopts the above-mentioned carbon-based composite material and its preparation method and application, and uses the catalyst generated by metal ions enriched in the biomass to grow carbon tubes on the surface of the carbon material, thereby increasing the specific surface area and conductivity of the carbon material and improving its electrochemical performance.
[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a carbon-based composite material, It is characterized in that The following steps are involved: S1. Dissolve the metal salt in deionized water, and stir with a magnetic stirrer until the metal salt is completely dissolved to obtain a metal salt solution; S2, immersing the biomass in a metal salt solution, utilizing the mineralization of the biomass to enrich the metal salt and realize self-assembly to obtain a precursor; S3, freeze-drying the precursor obtained in step S2 to obtain a sample; S4, pyrolyzing and carbonizing the sample in an argon atmosphere to obtain a carbon-metal composite material; S5, placing the carbon-metal composite material obtained in step S4 in an acidic solution to soak and remove excess metal particles, then washing with deionized water until neutral and placing in an oven for heat preservation to obtain carbonized biomass; S6, the biomass carbonized in step S5 is passed through sandpaper and a punch to obtain a carbon sheet; S7, further subjecting the carbon sheet obtained in step S6 to high-temperature carbonization, and placing melamine upstream thereof to generate a carbon-based composite material; In step S5, the acid solution is a hydrochloric acid solution with a concentration of 1-2 mol / L; the soaking time is 5-10 hours; the insulation time is 10-24 hours; and the insulation temperature is 50-80°C.
2. A method for preparing a carbon-based composite material according to claim 1, It is characterized in that In step S1, the mass ratio of metal salt to deionized water is 40-162:10000; the stirring temperature is 25°C; the stirring rate is 200-600 r / min; and the concentration of the metal salt solution is 0.05-0.2 mol / L.
3. A method for preparing a carbon-based composite material according to claim 1, It is characterized in that In step S2, the mass ratio of biomass to metal salt solution is 4-8:100; and the immersion time is 10-48 hours.
4. A method for preparing a carbon-based composite material according to claim 1, It is characterized in that In step S3, freeze drying is performed by keeping the mixture at -50°C for 1 to 5 hours and then drying the mixture at 20°C for 24 to 48 hours.
5. The method for preparing a carbon-based composite material according to claim 1, It is characterized in that In step S4, the carbonization temperature is 800-1000° C. and the carbonization time is 60 min.
6. The method for preparing a carbon-based composite material according to claim 1, It is characterized in that In step S6, the carbon sheet has a thickness of 0.55 to 0.65 mm and a diameter of 8 to 10 mm.
7. The method for preparing a carbon-based composite material according to claim 1, It is characterized in that In step S7, the high temperature carbonization process is to first increase the temperature to 180°C at 5°C / min and keep the temperature for 2h, and then increase the temperature to 680°C at 2°C / min and keep the temperature for 4h; The mass ratio of the carbon sheet to melamine is 1:240-400.
8. A carbon-based composite material prepared according to the method for preparing a carbon-based composite material according to any one of claims 1 to 7.
9. Use of the carbon-based composite material according to claim 8 in an alkali metal negative electrode carrier.
Citation Information
Patent Citations
Method for preparing negative electrode material of metal ion battery by taking bacteria as substrate, and battery
CN106920986A
Microbial enrichment preparation method of hypha-based doped supercapacitor material
CN111613456A
Method for constructing composite material based on bean sprouts
CN112735857A
Biological carbon material derived from waste edible fungus mycorrhiza and application of biological carbon material
CN115974046A
Biomass hard carbon composite negative electrode material and preparation method and application thereof
CN117613218A