A lithium-rich manganese-based positive electrode material with excellent low-temperature performance and a preparation method thereof

By adding surfactant to the spray solution, lithium-rich manganese oxide with small particle size is prepared, which solves the performance problem of lithium-rich manganese-based cathode materials in low-temperature environments, achieves efficient cycle performance and low-cost production, and is suitable for Electric vehicle applications in cold areas.

CN118026284BActive Publication Date: 2024-10-22XIAN TECH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410168926.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2024-10-22
Estimated Expiration
2044-02-06

AI Technical Summary

Technical Problem

Lithium-rich manganese-based cathode materials have low initial specific capacity, poor cycle performance, and rapid capacity decline in low-temperature environments, which cannot meet the needs of use in cold areas. Existing improvement methods are complex in operation, high in cost, and low in efficiency, and cannot be commercialized.

Method used

By adding surfactant to the spray solution, the surface tension is reduced, the dispersion of the metal salt is improved, and a small particle size precursor is prepared. After sintering, a highly active and stable lithium-rich manganese oxide is formed to reduce the particle size. , improve the dynamic properties of lithium ions.

Benefits of technology

It significantly improves the low-temperature performance of lithium-rich manganese-based cathode materials, extends the capacity retention rate and voltage retention rate, reduces production costs, and achieves efficient cycle performance in low-temperature environments, making it suitable for electric vehicle applications in severe cold environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118026284B_ABST
    Figure CN118026284B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of positive electrode materials for lithium-ion batteries, and specifically relates to a lithium-rich manganese-based positive electrode material with excellent low-temperature performance and a preparation method thereof, comprising the following steps: Step 1, preparing raw materials for layered lithium-rich manganese oxide positive electrode materials; Step 2, adding the raw materials, chelating agents and surfactants of the positive electrode materials into deionized water to prepare a spray solution, and spraying to obtain a positive electrode precursor; Step 3, sintering the precursor to obtain a layered lithium-rich manganese oxide positive electrode active material. The present invention proposes for the first time to add a surfactant to the spray solution to prevent the generation of precipitation in the spray solution; it can effectively reduce the particle size of the precursor after spray granulation, improve the material stability and cycle performance, and can effectively inhibit the voltage decay problem of lithium-rich manganese-based positive electrode materials at low temperatures, and improve their low-temperature performance conductivity. At the same time, the preparation method is convenient and easy to operate, which reduces the production cost and can realize large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium-ion battery positive electrode materials, and specifically relates to a lithium-rich manganese-based positive electrode material with excellent low-temperature performance and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high energy storage density, environmental friendliness, and portability, and are favored by scientific researchers. Among them, the high energy density lithium-rich manganese layered oxide cathode has attracted great attention.

[0003] The lithium-rich manganese-based positive electrode material [xLiMO2-(1-x)Li2MnO3] has the characteristics of "three highs", high discharge capacity (~280 mAh / g), high median voltage (3.6 volts), and high mass specific energy density (greater than 500 Wh / kg). It is also low-cost, and the material synthesis and material preparation processes are relatively simple, and it is expected to become the next generation of power battery positive electrode materials. However, the low-temperature performance of lithium-rich manganese-based positive electrode materials is poor. In low-temperature environments (0℃~-30℃), the initial specific capacity is low and the voltage and capacity decay too quickly. The poor cycle performance cannot meet the use needs in cold areas.

[0004] At present, the methods for preparing lithium-rich manganese positive electrode materials mainly include liquid phase co-precipitation, sol-gel, hydrothermal method, solid phase ball milling method and spray pyrolysis method. The means to improve the low-temperature performance of batteries are mainly divided into three aspects: the first is to improve the low-temperature ionic conductivity of the electrolyte; the second is to control the size of the positive electrode material particles; the third is morphology design and surface coating of the material. For example, by coating with materials such as aluminum oxide, aluminum fluoride, and lithium phosphate, the grain boundary resistance of lithium ions is reduced while the release of lattice oxygen is inhibited; the hydrothermal synthesis method is used to obtain micron-spheres formed by the agglomeration of layered nanocrystals, and its special morphology effectively improves the low-temperature cycle performance. Although the above methods improve the low-temperature performance of lithium-rich manganese positive electrode materials, the above modification methods all have the problems of complex operation, high cost and low efficiency, and cannot achieve the goal of commercial application.

[0005] Therefore, developing materials with excellent low-temperature performance and seeking simple, efficient, low-cost and environmentally friendly preparation methods are very meaningful for realizing the commercial application of high-energy-density layered lithium-manganese-rich positive electrodes.

[0006] In the document with application number "2021103148369", "a method for preparing a nano-carbon-coated composite lithium iron phosphate low-temperature positive electrode material" is disclosed. This method realizes the nano-size of lithium iron phosphate particles through a composite lithium source, and at the same time, the carbon nanotube composite carbon source coats the lithium iron phosphate, and the iron source, lithium source, organic carbon source, and dispersant are pre-dispersed. After dispersion, carbon nanotube slurry is added, and then the precursor slurry is obtained by sand grinding. After spray drying and granulation, the precursor is placed in a protective atmosphere for low-temperature sintering, and finally the product is obtained after being crushed by an air flow mill. During its preparation process, a dispersant is added during coating. In this technical solution, the purpose of adding a dispersant is to disperse the organic carbon source to make the coating effect better. There are also documents that add a dispersant during metal doping, and its function is also to make the doping effect of metal oxides better. However, their core design concept is to carry out morphology design and surface coating of materials, and does not involve the change of particle size of lithium-rich manganese-based materials. The particle size of lithium-rich manganese-based materials is the key to determining the kinetic properties of lithium ions, especially in low-temperature environments. The existing larger particle size will limit the low-temperature kinetic properties of lithium ions. Therefore, the problem of the existing technology is that lithium-rich manganese-based materials still have low initial specific capacity and capacity in low-temperature environments, poor cycle performance at low temperatures, and fast capacity decay, resulting in the problem that the low-temperature performance is still not ideal. Summary of the invention

[0007] In order to solve the problem that lithium-rich manganese-based materials have low capacity, poor cycle performance, and rapid capacity decay in low temperature environments, resulting in unsatisfactory low temperature performance, the present invention provides a lithium-rich manganese-based positive electrode material with excellent low temperature performance and a preparation method thereof.

[0008] To achieve the above object, the specific technical scheme of the present invention is as follows: A method for preparing a lithium-rich manganese-based positive electrode material with excellent low-temperature performance comprises the following steps:

[0009] Step 1: prepare a raw material of a layered lithium-rich manganese oxide positive electrode material according to the general structural formula xLi2MnO3-(1-x)LiMO2, wherein M is selected from one or more of Ni, Co, Mn, Cr, Fe, Al, Y, Nb, Mo, and Ru, and 0≤x≤1;

[0010] Step 2: adding the raw material of the positive electrode material, the chelating agent and the surfactant into deionized water in a certain proportion to prepare a spray solution, and spraying to obtain a positive electrode precursor;

[0011] Step 3: Sintering the precursor to obtain a positive electrode active material layered lithium-rich manganese oxide.

[0012] Furthermore, in the above step 1, the surfactant is selected from one or more of cetyltrimethylammonium bromide (CTMAB), sodium dodecyl sulfate (SDS), di-long chain alkyl dimethyl ammonium chloride, polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), sodium carboxymethyl cellulose (CMC), and guar gum (GG).

[0013] Furthermore, in the above step 1, the surfactant is preferably selected from cetyltrimethylammonium bromide (CTMAB), polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), sodium carboxymethylcellulose (CMC)

[0014] Furthermore, the above surfactant is preferably selected from polyvinyl pyrrolidone (PVP).

[0015] Furthermore, in the above step 1, preferably, 0.5≤x≤0.7.

[0016] Furthermore, in the above step 1, in the raw material of the positive electrode material, the metal M is a soluble salt, including nitrate, sulfate and / or acetate.

[0017] Furthermore, in the above step 2, the mass of the surfactant accounts for 0.5-10% of the total mass of the deionized water.

[0018] Furthermore, in the above step 2, the concentration of the metal salt solution is 0.2-3 mol / L.

[0019] Furthermore, in the above step 2, preferably, the mass of the surfactant accounts for 1-8% of the total mass of the deionized water; the concentration of the metal salt solution is 0.2-1 mol / L; and the chelating agent is citric acid.

[0020] The above preparation method produces a lithium-rich manganese-based positive electrode material with excellent low-temperature performance.

[0021] Compared with the prior art, the advantages of the present invention are:

[0022] 1. The present invention proposes for the first time to add a surfactant to the spray solution. The surfactant can reduce the surface tension of the spray solution, improve the dispersibility of the solute metal salts, produce a dissolution-promoting and solubilizing effect, and prevent the aggregation and precipitation of metal salts in the spray solution. In the conventional operation of spraying, the solution with the added surfactant has better dispersibility, which can effectively reduce the particle size of the precursor after spray granulation, so that the metal salts contained in the precursor can reach the atomic level and are evenly mixed. The activity of the precursor with a small particle size is greatly improved due to the increase in the surface area. At the same time, the surfactant plays a certain steric hindrance role, decomposes during the sintering process, and prevents the continuous growth of particles during the high-temperature sintering process, and finally reduces the size of the primary particles of the lithium-rich manganese oxide after high-temperature sintering. The primary particles after sintering are small and have high crystallinity, which can greatly improve the material stability and cycle performance, thereby effectively improving the low-temperature performance of the positive electrode material.

[0023] 2. Evenly mixed precursors with smaller particle sizes can sinter out lithium-rich manganese-based positive electrode materials with smaller primary particles. The nitrogen elements contained in the surfactant and the original metal elements can act as the redox center of the redox pair, regulate the redox of the original lattice oxygen, accelerate lithium ion transmission, and improve the low-temperature capacity and cycle performance of the material.

[0024] 3. Since the lithium-rich manganese-based positive electrode material provided by the present invention has the characteristics of high activity and small particle size, it can solve the problems of capacity decay and low initial specific capacity of lithium-rich manganese-based positive electrode materials at low temperatures, and at the same time can effectively inhibit its voltage decay and have high conductivity.

[0025] 4. The preparation method is convenient and easy to operate, which reduces the production cost:

[0026] (1) The final product is prepared by one-step mixing spray and one-step sintering, which is a mature process with low price, simple and efficient;

[0027] (2) Since the solution is prepared in one go and a surfactant is added to prevent the metal salt from settling, a high-concentration spray solution can be prepared, thereby improving the spray efficiency and thus the overall preparation efficiency, reducing energy consumption while reducing the use of solvent deionized water, thereby reducing production costs.

[0028] 5. The invention has a wide range of applications: The invention innovatively uses a surfactant one-step spray drying method to prepare a layered lithium-rich manganese positive electrode precursor with a particle size of only about 3 microns. After sintering, the primary particle size is only 100-200nm, which is significantly reduced compared to particles without surfactant (300-500nm), shortening the distance of lithium ion transmission-migration. The low-temperature performance after improvement by the surfactant is improved, whether it is the first charge and discharge capacity or the first coulomb efficiency, the capacity retention rate has been significantly improved, effectively solving the practical problems of capacity attenuation and poor cycle performance of lithium-rich manganese in low temperature environments (0℃-30℃), making it possible to use electric vehicles in severe cold environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a scanning electron microscope (SEM) image of the cathode material precursor prepared in Example 1;

[0030] Figure 2 is a particle size distribution diagram of the positive electrode precursor prepared in Example 1 by laser particle size analyzer;

[0031] Figure 3 is a scanning electron microscope (SEM) image of the lithium-rich manganese oxide after sintering the precursor of Example 1;

[0032] Figure 4 is the XRD pattern of the lithium-rich manganese oxide prepared in Example 1;

[0033] Figure 5 (a) the first charge and discharge curve of the assembled battery of Example 1 at 0°C; (b) the 0.1C cycle performance curve;

[0034] Figure 6 This is the median voltage decay curve of the assembled battery of Example 1 cycled at 0°C and 0.1C rate;

[0035] Figure 7 is the first charge and discharge curve of the assembled battery of Example 1 at -30°C (a);

[0036] Figure 8 (a) first charge and discharge curve of the assembled battery of Example 2 at 0°C; (b) 0.1C cycle performance curve;

[0037] Fig. 9 This is the median voltage decay curve of the assembled battery of Example 2 cycled at 0°C and 0.1C rate;

[0038] Fig.10 is the first charge and discharge curve of the assembled battery of Example 2 at -30°C (a);

[0039] Fig.11 (a) The first charge and discharge curve of the battery assembled in Example 1 at 0°C; (b) The 0.1C cycle performance curve;

[0040] Fig.12 This is the median voltage decay curve of the assembled battery of Example 1 cycled at 0°C and 0.1C rate;

[0041] Fig.13 This is the first charge and discharge curve of the comparative assembled battery at -30°C (a);

[0042] Fig.14 This is a scanning electron microscope (SEM) image of the positive electrode material precursor prepared in Comparative Example 1;

[0043] Fig.15 This is the particle size distribution diagram of the positive electrode precursor prepared in Comparative Example 1 by laser particle size analyzer;

[0044] Fig.16 is a scanning electron microscope (SEM) image of the lithium-rich manganese oxide after sintering the precursor of Comparative Example 1;

[0045] Fig.17 This is the XRD pattern of the lithium-rich manganese oxide prepared in Comparative Example 1. Specific implementation plan

[0046] The specific implementation method of the present invention is further described below in conjunction with examples. It should be noted here that the specific implementation method described here is only for illustrating and explaining the present invention and is not intended to limit the scope of protection of the present invention.

[0047] Embodiment 1, a method for preparing a lithium-rich manganese-based positive electrode material with excellent low-temperature performance, specifically comprising the following steps:

[0048] Step 1: Choose the classic 0.5Li2MnO3-0.5LiNi 0.33 Co0.33Mn 0.33 O2 layered lithium-rich manganese cathode material, simplified as Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2, that is, weigh the corresponding metal salts in the molar ratio of Li, Ni, Co, and Mn of 1.2:0.13:0.13:0.54. In this embodiment, the metal salt is acetate; weigh 10g of surfactant polyvinyl pyrrolidone (PVP) for use.

[0049] Step 2: Dissolve the metal salt in 1L deionized water at a concentration of 0.2mol / L, add 0.3mol citric acid for chelation, and then mix polyvinylpyrrolidone (PVP) into the solution. Stir at 50°C for 2 hours, ultrasonicate for half an hour, and then send it into a spray dryer for spray granulation to obtain a positive electrode precursor.

[0050] Step 3: Collect the positive electrode precursor, put it into a muffle furnace, heat it to 1000°C at 3°C / min, and keep it warm for 10 minutes. During the sintering period, air is continuously blown in with a blower to obtain a lithium-rich manganese-based positive electrode material.

[0051] The positive electrode sheet was prepared using the lithium-rich manganese-based positive electrode material prepared in this embodiment, and its electrochemical performance was characterized by a 2025 button cell, which was assembled in an Ar-filled glove box with a water and oxygen content of less than 0.01ppm. The ratio of active material, conductive agent, and binder in the positive electrode material is 84.5:10.5:5. Metal Li sheet was used as the reference electrode and counter electrode, Celgard-2400 was used as the diaphragm, LiPF6 (1 mol / L) / EC+DEC+EMC (1:1:1) was used as the electrolyte, and the test voltage window was 2.0-4.8V. The battery was tested for electrochemical performance by constant current charge and discharge.

[0052] Comparative Example:

[0053] The process for preparing the lithium-rich manganese-based positive electrode material is basically the same as that in Example 1, except that no surfactant is added, and the process for preparing the positive electrode sheet is basically the same as that in Example 1, and the active materials in the positive electrode material, layered lithium-rich manganese oxide, superP, and CMC are mixed in a mass ratio of 84.5:10.5:5. The assembly and test conditions of the battery are the same as those in Example 1.

[0054] The cathode precursor prepared in step 2 of Example 1 was characterized, and the SEM image of the cathode precursor was as follows: Figure 1 As shown in the figure, the particle size distribution diagram after laser particle size analyzer detection is as follows Figure 2 From the figure, it can be seen that the particle size of the precursor is mainly distributed in the range of 0.5μm-10 microns, and D50 is 3.059μm, which is consistent with the observation data under the electron microscope. Compared with the positive electrode precursor sprayed without adding surfactant to the solution, the particle size is significantly reduced after using surfactant, the particles are complete and the distribution is more concentrated. (See Fig.14 and Fig.15 )

[0055] Figure 3 The lithium-rich manganese-based oxide formed by sintering the positive electrode precursor sprayed with surfactant has a natural fragmented shape. Compared with the sample sintered without adding surfactant to the solution, the primary particles are evenly distributed and the particle size is significantly reduced, within the range of 100-200nm. (See Fig.16 )

[0056] Figure 4 This is the XRD diagram of the layered lithium-rich manganese oxide after sintering. The diffraction peak of the classic lithium-rich phase shifts to the left, the diffraction angle becomes smaller, the lattice parameter becomes larger, and lithium ions are easier to escape and embed, which is beneficial to the battery cycle at low temperature.

[0057] Figure 5 This is the electrochemical performance diagram of the assembled battery in this example. Figure 5 The left figure is the first charge and discharge curve of the battery at a current density of 20 mAh / g at 0°C. Its first charge capacity is 318.28 mAh / g, the first discharge capacity is 210.4 mAh / g, and the first coulombic efficiency is 66.11%. Figure 5 The right figure is the cycle performance curve of the battery assembled in this embodiment at a current density of 20 mAh / g (0.1C) at 0°C. After 50 cycles, the capacity is maintained at 206.91 mAh / g, and the capacity retention rate exceeds 103.27%, showing excellent cycle stability.

[0058] Figure 6 This is a voltage decay trend diagram corresponding to 50 cycles of the battery assembled in this embodiment at a current density of 200 mA / g at 0° C. The median voltage after 50 cycles is 3.518 V, and the voltage retention rate is 98.95%.

[0059] Figure 7 This is the first cycle charge and discharge diagram of the battery assembled in this embodiment at a current density of 20 mAh / g at -30°C. Its first charge capacity is 120 mAh / g, its first discharge capacity is 68.6 mAh / g, and its first coulombic efficiency is 57%.

[0060] Example 2, a method for preparing a lithium-rich manganese-based positive electrode material with excellent low-temperature performance: the ratio of each metal salt in the spray solution is the same as that in Example 1. The difference is that 30g of surfactant polyvinyl pyrrolidone (PVP) is added to 1L of water. The sintering process is to heat the temperature to 900°C at 5°C / min in a muffle furnace and keep it warm for 12 hours. During sintering, air is continuously blown in with a blower. The ratio of active substance, conductive agent, and binder in the positive electrode material is 85:10:5, and the resulting positive electrode sheet is recorded as 30-LLRO positive electrode sheet.

[0061] The battery assembly and testing conditions were the same as in Example 1. Figure 8 The left figure is the first charge and discharge curve of the battery at 0°C and 20 mAh / g current density, with the first charge capacity of 314 mAh / g, the first discharge capacity of 200.9 mAh / g, and the first coulombic efficiency of 63.98%. The right figure is the cycle performance curve of the battery assembled in this embodiment at 0°C and 20 mAh / g current density (0.1C), with the capacity remaining at 198.79 mAh / g after 50 cycles, and the capacity retention rate reaching 98.95%, showing good cycle stability.

[0062] Fig. 9This is a voltage decay trend diagram corresponding to 50 cycles of the battery assembled in this embodiment at a current density of 200 mA / g at 0° C. The median voltage after 50 cycles is 3.48 V, and the voltage retention rate is 92.3%.

[0063] Fig.10 This is the first cycle charge and discharge diagram of the battery assembled in this embodiment at a current density of 20 mAh / g at -30°C. Its first charge capacity is 108 mAh / g, its first discharge capacity is 61 mAh / g, and its first coulombic efficiency is 56.1%.

[0064] Example 3, a method for preparing a lithium-rich manganese-based positive electrode material with excellent low-temperature performance:

[0065] The ratio of each metal salt in the spray solution is the same as that in Example 1. The difference is that 10 g of surfactant sodium carboxymethyl cellulose is added to 1 L of water and 10 g of cetyltrimethylammonium bromide (CTMAB) is added for coordinated dispersion.

[0066] Embodiment 4, a method for preparing a lithium-rich manganese-based positive electrode material with excellent low-temperature performance, specifically comprising the following steps:

[0067] Step 1: Select 0.6Li2MnO3-0.4LiNi 0.33 Co 0.33 Mn 0.33 O2 layered lithium-rich manganese positive electrode material, prepare the corresponding mixed salt solution according to the corresponding proportion, the metal salt in the mixed salt solution in this embodiment is nitrate; weigh 10g of surfactant polyvinyl pyrrolidone (PVP) for use.

[0068] Step 2: Dissolve the metal salt in 1L deionized water at a concentration of 1 mol / L, add 0.4 mol citric acid for chelation, mix sodium carboxymethyl cellulose (PVP) into the solution, stir at 50°C for 2 hours, ultrasonicate for half an hour, and then add to a spray dryer for spray granulation to obtain a positive electrode precursor.

[0069] Step 3: The manufactured positive electrode precursor is placed in a muffle furnace, heated to 900°C at 3°C / min, and kept warm for 15 hours. During the sintering period, air is continuously blown in with a blower to obtain a lithium-rich manganese-based positive electrode material.

[0070] Characterize the cathode material and precursor prepared in this example and assemble the battery for electrochemical testing

[0071] Fig.11The left figure is the first charge and discharge curve of the battery at 0°C and 20 mAh / g current density. Its first charge capacity is 305.18 mAh / g, its first discharge capacity is 191 mAh / g, and its first coulombic efficiency is 62.58%. The right figure is the cycle performance curve of the battery assembled in this embodiment at 0°C and 20 mAh / g current density (0.1C). After 50 cycles, the capacity is maintained at 175.96 mAh / g, and the capacity retention rate reaches 92.12%.

[0072] Fig.12 The voltage decay trend diagram corresponding to 50 cycles of the battery assembled in this embodiment at a current density of 200 mA / g at 0° C., the median voltage after 50 cycles is 3.41 V, and the voltage retention rate is 89.97%.

[0073] Fig.13 This is the first cycle charge and discharge diagram of the battery assembled in the comparative example at a current density of 20 mAh / g at -30°C. Its first charge capacity is 93.7 mAh / g, the first discharge capacity is 37.2 mAh / g, and the first coulombic efficiency is 39.7%.

[0074] Fig.14 This is the SEM image of the positive electrode precursor of the comparative example. Fig.15 This is the particle size distribution diagram after the laser particle size analyzer test. From the comparison of the two figures, it can be seen that the precursor particle size is mainly distributed in the range of 0.5μm-45μm, and D50 is 10.96μm. The particle size analyzer test results are basically consistent with the observation data under the electron microscope.

[0075] Fig.16 This is a scanning electron microscope (SEM) image of the lithium-rich manganese oxide after sintering the positive electrode precursor in the comparative example, and the primary particle size is between 200-500nm.

[0076] Fig.17 This is the XRD diagram of the lithium-rich manganese oxide after sintering without adding a surfactant in the comparative example. It can be seen that the peak shapes are consistent before and after adding the surfactant.

[0077] In summary, embodiment 1 is the best embodiment.

[0078] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a lithium-rich manganese-based positive electrode material with excellent low-temperature performance, characterized in that: The following steps are involved: Step 1: prepare a raw material of a layered lithium-rich manganese oxide positive electrode material according to the general structural formula xLi2MnO3-(1-x)LiMO2, wherein M is selected from one or more of Ni, Co, Mn, Cr, Fe, Al, Y, Nb, Mo, and Ru, 0.5≤x≤0.7, and a metal salt is a metal acetate as a raw material of the metal element; weigh 10 g of a surfactant polyvinyl pyrrolidone for use; Step 2: Dissolve the metal salt in 1L deionized water at a concentration of 0.2 mol / L, add 0.3 mol of citric acid for chelation, and then mix polyvinyl pyrrolidone into the solution. Stir at 50°C for 2 hours, ultrasonicate for half an hour, and then send it into a spray dryer for spray granulation to obtain a positive electrode precursor. Step 3: Collect the positive electrode precursor, put it into a muffle furnace, heat it to 1000°C at 3°C / min, and keep it warm for 10 minutes. During the sintering period, air is continuously blown in with a blower to obtain a lithium-rich manganese-based positive electrode material.

Citation Information

Patent Citations

  • Lithium-rich manganese-based material and preparation method thereof

    CN102956884A

  • Method for improving electrochemical properties of electrode material of lithium ion batteries

    CN107093726A