A high-entropy oxide ceramic solar thermal material with multiple components
By doping rare earths and transition metals into perovskite structures, high-entropy oxide ceramic materials are solved, and the problem of insufficient photothermal efficiency and thermal stability of existing solar photothermal materials is achieved, and efficient solar energy absorption and high temperature stability are achieved. , suitable for a variety of renewable energy applications.
Patent Information
- Application Number
- CN202410271594.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing solar photothermal materials have shortcomings in photothermal efficiency and thermal stability, especially in high temperature conditions, which are difficult to meet the needs of concentrated solar systems.
Using high-entropy oxide ceramic materials with super many components, the perovskite structure is formed through multi-element doping of rare earth elements and transition metals, and the photothermal absorption capacity and high temperature stability of the material are improved by using high-entropy strategies. The specific preparation is made The methods include ball mill mixing and high temperature calcining.
The solar energy absorption rate in the 0.3~2.5μm band is significantly improved, and the material maintains absorption stability under 900℃. It has excellent high-temperature thermal stability and anti-oxidation and corrosion resistance. It is suitable for solar photothermal power generation and seawater desalination and other fields. .
Smart Images

Figure CN118026682B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar thermal materials, and in particular to a high-entropy oxide ceramic solar thermal material with super-multi-components. Background Art
[0002] With the continuous depletion of fossil fuels and the increasing prominence of environmental problems, the application of renewable energy is particularly important. As a clean and renewable energy, solar energy has been widely used in various fields of life and plays an increasingly important role. The penetration of renewable energy such as photovoltaics and wind power in the power grid is increasing, and its intermittency and stability issues are becoming a huge challenge. Concentrated solar thermal power generation is considered to be an attractive solution that can provide stable, dispatchable and cheap power generation from renewable solar energy. In addition, the freshwater crisis has a profound impact on human well-being and global sustainable development. Exploring unconventional water resources has become a viable solution to alleviate freshwater shortages, among which solar evaporation is a zero-energy and environmentally friendly method of obtaining freshwater. In these applications, solar thermal materials play a vital role and determine the photothermal efficiency of the materials. Materials with broadband absorption capacity can bring considerable economic benefits. For concentrated solar energy systems, materials are required not only to have excellent solar absorption capacity, but also to have good thermal stability to increase working life and operation cycle.
[0003] Perovskite ABO3 type high entropy ceramic components have the characteristics of large adjustable space and high oxygen vacancy concentration, and have strong competitive advantages in ceramic materials for new thermal protective coatings. This type of high entropy ceramic can be regulated by high entropy components at two sites, A and B, separately or simultaneously, so that there is severe lattice distortion in the unit cell, showing high mass disorder, ion size disorder and charge disorder. These special effects can significantly improve the comprehensive performance of the material, making it exhibit excellent molten salt corrosion resistance, high temperature phase stability and mechanical properties. In addition, when A and B are doped with multiple elements, anion defects are easily formed or cations show different valence states, which can enhance free carrier absorption and improve the solar energy absorption capacity of the material system. In addition, high entropy ceramics have high configurational entropy, and the entropy-driven structural stabilization effect can allow super-multiple cationic components to be doped in the perovskite structure. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a high-entropy oxide ceramic solar thermal material with excellent photothermal absorption capacity and super-multi-components.
[0005] To solve the above problems, the present invention discloses a high-entropy oxide ceramic solar thermal material with super-multi-components, characterized in that: the chemical formula of the solar thermal material is ABO3; the A position is any five elements among the rare earth elements La, Nd, Sm, Ce, Pr, and Gd, and the cation has a 12-coordinate structure, coordinated with 12 oxygen atoms, and is located in a cavity formed by an octahedron; B is any five elements among the transition metal elements Mn, Fe, Al, Cr, Co, and Ni, and the cation forms an octahedral coordination with six oxygen ions.
[0006] The solar thermal material has a solar absorption rate of 0.83-0.88 in the 0.3-2.5 μm band.
[0007] The method for preparing a high-entropy oxide ceramic solar thermal material with super-multi-components as described above is characterized in that: the method refers to La2O3, Nd2O3, Sm2O3, Ce2O3, Pr6O 11 , Gd2O3 and any five powders of MnO2, Fe2O3, Al2O3, Cr2O3, Co2O3, and Ni2O3 are used as raw materials, and ball milling is carried out to mix them according to a metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1, and a mixture powder is obtained after drying and grinding; the mixture powder is calcined at high temperature in a muffle furnace, and after cooling and grinding, the solar thermal material is obtained.
[0008] The ball milling mixing conditions refer to using a planetary ball mill for wet ball milling, the ball milling speed is 300-500 r / min, the ball milling time is 12-24 hours, and the mass ratio of the ball material to anhydrous ethanol is 2-4:1:3.
[0009] The high temperature calcination conditions refer to a calcination temperature of 1000-1600° C., a heating rate of 3-5° C. / min, and a calcination time of 4-8 hours.
[0010] The cooling method is one of furnace cooling, air quenching cooling and liquid nitrogen quenching cooling.
[0011] Compared with the prior art, the present invention has the following advantages:
[0012] 1. The present invention forms an impurity energy level between the top of the valence band and the bottom of the conduction band by doping the perovskite structures A and B with multiple transition metal and rare earth metal cations of different valence states and valence bond structures at the same time, thereby enhancing the free carrier (electron, hole, etc.) concentration and inter-band transition in the valence band, thereby having an excellent solar energy absorption rate. At the same time, such cations of different valence states will also generate oxygen vacancies, forming intermediate energy levels, and enhancing the solar energy absorption capacity.
[0013] 2. The present invention uses a high entropy strategy to modify traditional perovskite ceramics, giving them excellent light and heat absorption capabilities, with a solar absorptivity of 0.83-0.88 in the 0.3-2.5 μm band. At the same time, the material also has excellent high-temperature thermal stability. After annealing at 900°C for 24 hours, the material's absorptivity decreases by less than 0.02. Therefore, the material can be used in solar thermal power generation, seawater desalination, solar water heaters and other fields.
[0014] 3. The ultra-multi-component mixing of the present invention significantly improves the material configuration entropy, which is beneficial to reduce the Gibbs free energy, so that the material exhibits entropy-driven structural stability characteristics, has good high-temperature stability and anti-oxidation and anti-corrosion capabilities. At the same time, doping ultra-multi-components in a single-phase solid solution structure provides abundant space for optimizing material performance.
[0015] 4. The present invention is simple to operate, has high production efficiency, does not require complicated post-processing, and can be used for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The specific implementation modes of the present invention will be further described in detail below in conjunction with the accompanying drawings.
[0017] Figure 1 For Example 1 of the present invention (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )XRD pattern of O3.
[0018] Figure 2 Example 2 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )XRD pattern of O3.
[0019] Figure 3 Example 2 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr0.2 Co 0.2 )SEM image of O3.
[0020] Figure 4 Example 2 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 ) Solar absorption spectrum of O3 in the 0.3~2.5μm band.
[0021] Figure 5 Example 3 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )XRD pattern of O3.
[0022] Figure 6 For Example 4 of the present invention (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )XRD pattern of O3. DETAILED DESCRIPTION
[0023] A high entropy oxide ceramic solar thermal material with super-multi-components, the chemical formula of the solar thermal material is ABO3; the A position is any five elements among the rare earth elements La, Nd, Sm, Ce, Pr, and Gd, the cation is in a 12-coordinate structure, coordinated with 12 oxygen atoms, and located in a cavity formed by an octahedron; B is any five elements among the transition metal elements Mn, Fe, Al, Cr, Co, and Ni, the cation forms an octahedral coordination with six oxygen ions. The solar thermal material has a solar absorptivity of 0.83-0.88 in the 0.3-2.5 μm band.
[0024] Its preparation method: This method refers to La2O3, Nd2O3, Sm2O3, Ce2O3, Pr6O 11Any five powders of Gd2O3 and any five powders of MnO2, Fe2O3, Al2O3, Cr2O3, Co2O3, and Ni2O3 are used as raw materials, and a planetary ball mill is used for wet ball milling according to a metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1, the ball milling speed is 300-500r / min, the ball milling time is 12-24 hours, and the mass ratio (g / g) of the ball material to anhydrous ethanol is 2-4:1:3. After ball milling and mixing, the mixture is dried at 80-100℃, and then ground to obtain a mixture powder; the mixture powder is calcined at high temperature in a muffle furnace, the calcination temperature is 1000-1600℃, the heating rate is 3-5℃ / min, and the calcination time is 4-8 hours. After calcination, it is cooled to room temperature by one of furnace cooling, air quenching cooling, and liquid nitrogen quenching cooling, and finally ground to obtain a solar thermal material.
[0025] Example 1 A method for preparing a high entropy oxide ceramic solar thermal material with multiple components:
[0026] According to the metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1:1, La2O3 (1 mol), Nd2O3 (1 mol), Sm2O3 (1 mol), Ce2O3 (1 mol), Gd2O3 (1 mol), MnO2 (1 mol), Fe2O3 (1 mol), Al2O3 (1 mol), Cr2O3 (1 mol), and Co2O3 (1 mol) powders were weighed as raw materials respectively; according to the mass ratio (g / g) of ball material to anhydrous ethanol of 2:1:3, zirconia balls, raw materials and anhydrous ethanol were poured into a planetary ball mill respectively, and ball milling was carried out for 1 hour at a speed of 300 r / min, followed by a pause of 10 minutes, which was a ball milling cycle. After 10 minutes, ball milling was carried out again for 1 hour at a speed of 300 r / min, for a total of 24 hours. After ball milling, the mixture was dried at 80-100°C and then ground to obtain a mixture powder. The mixture powder was calcined in a muffle furnace at a high temperature of 1000°C, a heating rate of 3°C / min, and a calcination time of 8 hours. After calcination, it was quenched in liquid nitrogen and cooled to room temperature. Finally, it was ground to obtain a single-phase (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )O3 solar thermal materials.
[0027] Figure 1 As described in Example 1 (La 0.2 Nd0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )O3 solar thermal material XRD pattern, the spectrum line and the ICDD database with perovskite structure of LaCoO3 spectrum line (PDF#75-0279) are very consistent, indicating that the solar thermal material prepared in this example is a perovskite structure.
[0028] For income (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )O3 solar thermal material for photothermal performance and thermal stability evaluation:
[0029] Test method: A Lambda 950 UV / visible / near-infrared spectrophotometer (equipped with a 150 mm integrating sphere) manufactured by PerkinElmer, USA, was used to evaluate the solar thermal performance of the solar thermal material. Its reflectance spectrum in the 0.3-2.5 μm band was measured, and then the solar light absorption rate in this band was calculated according to formula (1).
[0030]
[0031] Where: α(θ, λ) is the absorptivity of the material at the solar incident angle θ and wavelength λ; R(θ,λ) is the reflectivity of the material at the solar incident angle θ and wavelength λ; I S (λ) is the spectral radiation intensity of the sun when the atmospheric mass is AM 1.5.
[0032] The prepared solar thermal material was placed in an air atmosphere in a box furnace and a thermal stability experiment was carried out at 900°C for 24 hours.
[0033] The test sample amount is 0.2g.
[0034] The results showed that the solar light absorption rate of the solar thermal material in the 0.3~2.5μm band was 0.859; after the thermal stability experiment, the solar light absorption rate of the solar thermal material in the 0.3~2.5μm band was measured to be 0.845.
[0035] Example 2 A method for preparing a high entropy oxide ceramic solar thermal material with multiple components:
[0036] According to the metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1, La2O3 (1 mol), Nd2O3 (1 mol), Sm2O3 (34.872 g), Ce2O3 (1 mol), Pr6O 11 (1mol), MnO2 (1mol), Fe2O3 (1mol), Al2O3 (1mol), Cr2O3 (1mol), Co2O3 (1mol) powders are used as raw materials; according to the mass ratio of ball material to anhydrous ethanol (g / g) of 3:1:3, the zirconia balls, raw materials and anhydrous ethanol are poured into a planetary ball mill respectively, and ball milling is carried out for 1 hour at a speed of 300r / min, followed by a pause of 10min, which is a ball milling cycle. After 10min, ball milling is carried out again for 1 hour at a speed of 300r / min, for a total of 24 hours of ball milling. After ball milling, the mixture is dried at 80~100℃, and then ground to obtain a mixture powder; the mixture powder is calcined at high temperature in a muffle furnace, the calcination temperature is 1400℃, the heating rate is 3℃ / min, and the calcination time is 4 hours. After calcination, it is air quenched and cooled to room temperature, and ground to obtain a single-phase (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )O3 solar thermal materials.
[0037] Figure 2 As described in Example 2 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )O3 solar thermal material XRD pattern, the spectrum line and the ICDD database with perovskite structure LaAlO3 spectrum line (PDF#75-4121) are very consistent, indicating that the solar thermal material prepared in this example is a single-phase solid solution of perovskite structure.
[0038] For income (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Co 0.2 )O3 solar thermal material was used to evaluate the photothermal performance and thermal stability. The test method and test sample dosage were the same as in Example 1.
[0039] The results show that the solar thermal material has a solar light absorption rate of 0.875 in the 0.3~2.5μm band. Figure 3 As shown, it indicates that the solar thermal material has a higher solar thermal rate in this band.
[0040] After thermal stability tests, the solar thermal material was found to have a solar light absorption rate of 0.873 in the 0.3-2.5 μm band. Figure 4 As shown, no phase change occurred after the thermal stability experiment at 1500°C, indicating that the solar thermal material has good thermal stability.
[0041] Example 3 A method for preparing a high entropy oxide ceramic solar thermal material with multiple components:
[0042] According to the metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1:1, La2O3 (1 mol), Nd2O3 (1 mol), Sm2O3 (1 mol), Ce2O3 (1 mol), Gd2O3 (1 mol), MnO2 (1 mol), Fe2O3 (1 mol), Al2O3 (1 mol), Cr2O3 (1 mol), and Ni2O3 (1 mol) powders were weighed as raw materials respectively; according to the mass ratio (g / g) of ball material to anhydrous ethanol of 4:1:3, zirconia balls, raw materials and anhydrous ethanol were poured into a planetary ball mill respectively, and ball milling was carried out for 1 hour at a speed of 500 r / min, followed by a pause of 10 minutes, which was one ball milling cycle. After 10 minutes, ball milling was carried out again for 1 hour at a speed of 500 r / min, for a total of 10 hours. After ball milling, the mixture was dried at 80-100°C and then ground to obtain a mixture powder; the mixture powder was calcined in a muffle furnace at a high temperature of 1400°C, a heating rate of 3°C / min, and a calcination time of 4 hours. After calcination, the mixture was cooled to room temperature and ground to obtain a single-phase (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )O3 solar thermal materials.
[0043] Figure 5 As described in Example 3 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )O3 solar thermal material XRD pattern, the spectrum line and the ICDD database with perovskite structure LaAlO3 spectrum line (PDF#75-4121) are very consistent, indicating that the solar thermal material prepared in this embodiment is a single-phase solid solution of perovskite structure.
[0044] For income (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 G 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )O3 solar thermal material was used to evaluate the photothermal performance and thermal stability. The test method and test sample dosage were the same as in Example 1.
[0045] The results show that the solar light absorption rate of the solar thermal material in the 0.3~2.5μm band is 0.833; after the thermal stability experiment, the solar light absorption rate of the solar thermal material in the 0.3~2.5μm band was measured to be 0.830.
[0046] Example 4 A method for preparing a high entropy oxide ceramic solar thermal material with multiple components:
[0047] According to the metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1, La2O3 (1 mol), Nd2O3 (1 mol), Sm2O3 (34.872 g), Ce2O3 (1 mol), Pr6O 11(1mol), MnO2 (1mol), Fe2O3 (1mol), Al2O3 (1mol), Cr2O3 (1mol), Ni2O3 (1mol) powders are used as raw materials; according to the mass ratio of ball material to anhydrous ethanol (g / g) of 3:1:3, the zirconia balls, raw materials and anhydrous ethanol are poured into a planetary ball mill respectively, and ball milling is performed for 1 hour at a speed of 400r / min, followed by a pause of 10min, which is a ball milling cycle. After 10min, ball milling is performed for another hour at a speed of 400r / min, for a total of 12 hours of ball milling. After ball milling, the mixture is dried at 80~100℃, and then ground to obtain a mixture powder; the mixture powder is calcined at high temperature in a muffle furnace, the calcination temperature is 1600℃, the heating rate is 5℃ / min, and the calcination time is 4 hours. After calcination, it is air quenched and cooled to room temperature, and ground to obtain a single-phase (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )O3 solar thermal materials.
[0048] Figure 6 As described in Example 4 (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )O3 solar thermal material XRD pattern, the spectrum line and the ICDD database with perovskite structure LaAlO3 spectrum line (PDF#75-4121) are very consistent, indicating that the solar thermal material prepared in this example is a single-phase solid solution of perovskite structure.
[0049] For income (La 0.2 Nd 0.2 Sm 0.2 Ce 0.2 Pr 0.2 )(Mn 0.2 Fe 0.2 Al 0.2 Cr 0.2 Ni 0.2 )O3 solar thermal material was used to evaluate the photothermal performance and thermal stability. The test method and test sample dosage were the same as in Example 1.
[0050] The results show that the solar light absorption rate of the solar thermal material in the 0.3~2.5μm band is 0.850; after the thermal stability experiment, the solar light absorption rate of the solar thermal material in the 0.3~2.5μm band was measured to be 0.845.
[0051] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. All changes made within the scope of protection of the independent claims of the present invention are within the scope of protection of the present invention.
Claims
1. A high entropy oxide ceramic solar thermal material with multiple components, characterized in that: The chemical formula of the solar thermal material is ABO3; the A position is the rare earth elements La, Nd, Sm, Ce and Pr, or the A position is the rare earth elements La, Nd, Sm, Ce and Gd, the cation is in a 12-coordinate structure, coordinated with 12 oxygen atoms, and located in a cavity formed by an octahedron; B is the metal elements Mn, Fe, Al, Cr and Co, or B is the metal elements Mn, Fe, Al, Cr and Ni, the cation forms an octahedral coordination with six oxygen ions; the solar thermal material has a solar absorptivity of 0.83-0.88 in the 0.3-2.5 μm band; the preparation method of the solar thermal material is to prepare a 12-coordinate structure of La2O3, Nd2O3, Sm2O3, Ce2O3 and Pr6O 11 Five powders or five powders of La2O3, Nd2O3, Sm2O3, Ce2O3 and Gd2O3, and five powders of MnO2, Fe2O3, Al2O3, Cr2O3 and Co2O3 or five powders of MnO2, Fe2O3, Al2O3, Cr2O3 and Ni2O3 are used as raw materials, ball milling and mixing are carried out according to a metal atomic molar ratio of 1:1:1:1:1:1:1:1:1:1, and a mixture powder is obtained after drying and grinding; the mixture powder is calcined at high temperature in a muffle furnace, and then cooled and ground to obtain solar thermal material; the ball milling mixing conditions are as follows: wet ball milling is carried out using a planetary ball mill, the ball milling speed is 300-500 r / min, the ball milling time is 12-24 hours, and the mass ratio of ball material to anhydrous ethanol is 2-4:1:
3.
2. A high entropy oxide ceramic solar thermal material with super-multi-components as claimed in claim 1, characterized in that: The high temperature calcination conditions refer to a calcination temperature of 1000-1600° C., a heating rate of 3-5° C. / min, and a calcination time of 4-8 hours.
3. A high entropy oxide ceramic solar thermal material with super-multi-components as claimed in claim 1, characterized in that: The cooling method is one of furnace cooling, air quenching cooling and liquid nitrogen quenching cooling.
Citation Information
Cited By
High-entropy perovskite and lanthanum zirconate eutectic infrared ceramic, preparation method and application thereof
CN122958171A