A five-layer co-extruded biodegradable barrier film and its preparation method and application
Through the double-layer sandwich structure and co-extrusion processing technology of the five-layer co-extrusion biodegradable barrier film, the problems of the existing barrier materials in recycling and processing performance are solved, and efficient and environmentally friendly packaging materials are achieved to meet a variety of application needs.
Patent Information
- Application Number
- CN202410111533.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-25
AI Technical Summary
Existing barrier materials have problems in recycling and environmental protection, and are costly and poorly processed, which limits their application, especially PVA materials have challenges in thermoplastic processing.
Five layers of coextruded biodegradation barrier film are used, and a double-layer sandwich structure is adopted, including modified biodegradable materials, thermoplastic polyvinyl alcohol PVA material and PBAT-PVAlike-based fat-aromatic copolyester as bonding layers, through coextrusion Processing technology is prepared, combining catalyst and filler to improve bonding and barrier properties.
It achieves high oxygen and water resistance, good mechanical, sealing and weather resistance, low cost, suitable for food, medical medicine and electronic packaging, and is easy to industrially produce.
Smart Images

Figure CN118027366B_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of biodegradable material flexible packaging, and in particular to a five-layer co-extruded biodegradable barrier film and a preparation method and application thereof. Background technology:
[0002] Barrier materials can be used as interlayer films and other materials to form composite materials, or as coatings applied to other materials. Currently, there are mainly PVA, PVDC, EVOH, PA, aluminum-containing materials, etc., but metal-containing materials and halogen-containing materials are not conducive to recycling and environmental protection. EVOH is mainly imported and expensive. PA or PET and other materials have poor processing performance during blow molding, which greatly limits their application and causes waste of resources. PVA is a water-soluble, degradable material with low cost and excellent oxygen barrier performance. If its thermoplastic processing problem is solved, it will be an ideal oxygen barrier layer material. Summary of the invention:
[0003] In order to overcome the above-mentioned problems existing in the prior art, the present invention provides a five-layer co-extruded biodegradable barrier film and a preparation method and application thereof. The five-layer co-extruded biodegradable barrier film proposed in the present invention adopts a double-layer sandwich structure. The composite film adopting this structure not only has high oxygen and water barrier properties, but also has good mechanical properties, sealing properties, heat sealing properties and weather resistance, etc. In addition, the composite film has low cost and can meet the packaging requirements for food, medical drugs, electronic products, etc.
[0004] The first object of the present invention is to provide a biodegradable fat-aromatic copolyester based on "PBAT-PVAlike", the structural formula of which is shown in formula (I):
[0005]
[0006] In formula (I), 2≤m≤7, 1:1≤x:y≤1:1.3, and the number average molecular weight is 23000-28100 g / mol.
[0007] Preferably, the biodegradable aliphatic-aromatic copolyester has a number average molecular weight of 23970-28020 g / mol and a molecular weight distribution PDI of 1.70-1.81.
[0008] The second object of the present invention is to provide a method for preparing the biodegradable fat-aromatic copolyester based on "PBAT-PVAlike", comprising the following steps:
[0009] S1. Normal pressure esterification reaction: terephthalic acid, adipic acid, triol and catalyst I are added to a reaction vessel, the sum of the molar amounts of terephthalic acid and adipic acid is taken as the molar amount of the total acid, the amount of catalyst I is 0.1%-0.25% of the molar amount of the total acid, the molar ratio of triol to total acid is 1.1:1-1.7:1, the molar ratio of terephthalic acid to adipic acid is 1:1, and the temperature is gradually raised to 180°C-210°C under normal pressure and inert atmosphere, and the water fraction is collected. The esterification reaction is judged to be finished when the esterification water output reaches 95% or more of the theoretical value;
[0010] S2. Vacuum polycondensation reaction: Add catalyst II to the reaction vessel in an amount of 0.35%-0.45% of the molar amount of the total acid, gradually reduce the pressure and increase the temperature, evacuate to below 200 Pa, increase the temperature to 200°C-230°C, and carry out polycondensation dealcoholization reaction. The entire polycondensation reaction lasts for 2.5-3h, and then the reactor is filled with N2 to normal pressure to obtain the target product.
[0011] The biodegradable fat-aromatic copolyester proposed in the present invention contains the molecular chain segment structure of polyester and PVA at the same time, the main chain contains ester groups, and the side chains contain characteristic functional groups such as hydroxyl groups, and has both biodegradability and excellent bonding properties. The copolymer is not only similar to the biodegradable resin structure containing ester groups such as PBAT, PLA, PBS, PPC, PBST, etc., and has good bonding properties; the polyhydroxyl groups introduced in the side chains can produce hydrogen bonds with the hydroxyl groups on the PVA chain, greatly improving the bonding properties with the PVA sheet; it can perfectly meet the bonding performance requirements between the modified biodegradable material and the PVA material.
[0012] Preferably, the tribasic acid in step S1 is 1,2,4-butanetriol, pentane-1,2,5-triol (1,2,5-pentanetriol), 1,2,6-hexanetriol, heptane-1,2,7-triol (1,2,7-heptanetriol), octane-1,2,8-triol (1,2,8-octantriol) or nonane-1,2,9-triol (1,2,9-nonanetriol), and the catalyst I is tetrabutyl titanate (Ti(OC4H9)4) or ethylene glycol titanium ((C4H 10 O2)Ti); the catalyst II described in step S2 is tetrabutyl titanate (Ti(OC4H9)4), ethylene glycol titanium ((C4H 10 O2)Ti) or tetrabutyl titanate / trimethyl phosphate ((CH3O)3PO).
[0013] More preferably, the amount of catalyst I is 0.15% of the total acid molar amount, the molar ratio of triol to total acid is 1.3:1-1.5:1, and the amount of catalyst II is 0.4% of the total acid molar amount.
[0014] In the synthesis process of aliphatic-aromatic copolyesters, the most commonly used catalyst is polyester titanium catalyst, which has the characteristics of high activity, low price, no heavy metal, non-toxic and environmentally friendly.
[0015] The polyester condensation polymerization reaction is a chain growth reaction based on the chelate coordination mechanism. During the reaction, the lone pair of electrons provided by the O atom in the ester carbonyl group coordinates with the empty orbital provided by the metal center to increase the positive charge of the C atom in the carbonyl C=O and reduce the activation energy of the transition state. During the condensation polymerization, the O in the hydroxyl oxygen attacks the carbonyl C atom and combines with it, and performs directional polymerization of insertion growth like a template, thereby completing the condensation reaction.
[0016] The electron-donating P=O group in phosphate compounds can provide electron pairs as a thermal stabilizer, coordinate with the empty orbital of the metal center to reduce the activity of thermal degradation reactions, thereby achieving the purpose of reducing thermal degradation reactions. In addition, phosphates (such as trimethyl phosphate) can also undergo ester exchange reactions with the alcohol hydroxyl groups at the end of the chain, playing a capping role and preventing the chain end from degradation.
[0017] The third object of the present invention is to provide the application of the biodegradable aliphatic-aromatic copolyester based on "PBAT-PVAlike" in bonding composite films.
[0018] The biodegradable fat-aromatic copolyester based on "PBAT-PVAlike" proposed in the present invention has excellent bonding properties with PBAT, PLA, PBS, PPC, PBST film layers and PVA film layers containing ester structures, and can be used as a binder for the composite film composed of the above-mentioned film layers.
[0019] The fourth object of the present invention is to provide a five-layer co-extruded biodegradable barrier film, which is composed of ABCBA layers; the A layer is a modified biodegradable material, the C layer is a high oxygen barrier PVA material, and the B layer is the biodegradable fat-aromatic copolyester based on "PBAT-PVA like" as described in claim 1 or the biodegradable fat-aromatic copolyester based on "PBAT-PVA like" obtained by the preparation method as described in claim 3, and the total thickness of the B layer is 10%-30% of the total thickness of the five-layer co-extruded high barrier film.
[0020] The composite film adopts a double-layer sandwich structure, with layer A accounting for 30%-40% of the total thickness of the film, layer C accounting for 10%-40% of the total thickness of the film, and layer B accounting for 20%-60% of the total thickness of the film. The total thickness of the biodegradable barrier film proposed by the present invention is preferably 50 μm.
[0021] Preferably, the modified biodegradable material is obtained by filling a barrier filler in a base resin, the base resin is selected from one or more of PBAT, PLA, PBS, PPC, PBST, and the barrier filler is talcum powder, montmorillonite or mica. The modified biodegradable material is obtained by mixing the base resin and the barrier filler.
[0022] The composition of the modified biodegradable material is as follows: 100 parts of base resin and 1-40 parts of barrier filler by weight. The melt index of the modified biodegradable material is 1-5 g / 10 min.
[0023] Preferably, the high oxygen barrier PVA material is prepared by the following steps: PVA, flow regulator, and processing stabilizer are mixed evenly, then the temperature is raised to 70°C-90°C, stirring is continued, and the plasticizer is slowly added. After the addition is completed, stirring is continued for 8-12 minutes, and then the material is discharged, and then extruded and granulated by a twin-screw extruder to obtain the high oxygen barrier PVA material.
[0024] The PVA is preferably polyvinyl alcohol with an alcoholysis degree of 88, such as at least one of 0588, 1788, and 2488. The plasticizer is preferably glycerol or a glycol auxiliary agent, the flow regulator is preferably white carbon black, and the processing stabilizer is preferably hydrotalcite (1250 mesh).
[0025] The composition of each component in the high oxygen barrier PVA material is as follows: by mass: 100 parts of polyvinyl alcohol, 25-35 parts of plasticizer, 0.3-2.0 parts of flow regulator, and 0.3-2.0 parts of processing stabilizer.
[0026] The fifth object of the present invention is to provide a method for preparing the five-layer co-extruded biodegradable barrier film, wherein the biodegradable barrier film is obtained by five-layer co-extrusion blow molding, and the method specifically comprises the following steps: conveying the materials of layer A, layer B and layer C to a five-layer co-extrusion film blowing unit, wherein the extrusion temperature of layer A is 175°C to 185°C, the extrusion temperature of layer B is 175°C to 185°C, the extrusion temperature of layer C is 180°C to 190°C, the temperature of the die head is 170°C to 180°C, the extruded material is blown through the die to form a five-layer co-extruded biodegradable barrier film, and the pulling speed after co-extrusion is 2.0-7.5m / min.
[0027] Preferably, the extrusion temperature of layer A is 180°C, the extrusion temperature of layer B is 180°C, the extrusion temperature of layer C is 185°C, and the die head mold temperature is 175°C.
[0028] The sixth object of the present invention is to provide the use of the five-layer co-extruded biodegradable barrier film as a biodegradable packaging material. The composite film proposed by the present invention not only has high oxygen and water barrier properties, but also has good mechanical properties, sealing properties, heat sealing properties and weather resistance, etc. In addition, the composite film has low cost and can meet the packaging requirements for food, medical drugs, electronic products, etc.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] 1. The five-layer co-extruded biodegradable barrier film prepared by the present invention has a barrier layer C made of thermoplastic polyvinyl alcohol (PVA) material, which is not only biodegradable, but also has a simple preparation method and is easy to industrialize and mass produce.
[0031] 2. The B-layer adhesive layer used in the present invention is a copolyester containing a molecular segment structure of polyester and PVA, and has excellent adhesion when used as an adhesive layer. This polyester is not only similar in structure to biodegradable materials such as PBAT, PLA, PBS, PPC, PBST, etc. containing an ester structure, but also has good compatibility; the newly introduced polyhydroxyl groups in the side chain can produce hydrogen bonds with the hydroxyl groups on the PVA chain, greatly improving the adhesion with the PVA sheet; it can significantly improve the interfacial compatibility of the A-layer and the C-layer, and can perfectly meet the bonding performance requirements of different biodegradable materials such as PBAT / PVA multifunctional composite materials. At the same time, it also greatly improves the stability of the composite film structure of different biodegradable materials such as PBAT / PVA. Compared with commercially available binders such as EVA and maleic anhydride grafted polyethylene, the B-layer resin of the present invention also has a biodegradable function, which improves the mechanical properties and biodegradability of the biodegradable barrier film.
[0032] 3. The present invention can flexibly obtain a five-layer co-extruded film with adjustable and controllable barrier properties by designing the composition of the five-layer co-extruded film A, B, and C layers and controlling the co-extrusion processing traction speed. Description of the drawings:
[0033] Figure 1 This is the infrared spectrum of the copolymer adhesive resin B1 obtained in Example 1. Specific implementation method:
[0034] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0035] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.
[0036] The five-layer co-extruded biodegradable barrier film proposed in the present invention adopts a double-layer sandwich structure. The thickness of the A layer and the B layer on both sides are adjusted according to actual conditions. In the following embodiments, the thickness of the A layer or the B layer on both sides is equal.
[0037] Example 1
[0038] This embodiment provides a five-layer co-extruded biodegradable barrier film 1, and the preparation method thereof is as follows:
[0039] (1) Preparation of A1 layer material: The mass ratio of PBAT to montmorillonite is 100:1, and the melt index of the composite material is 5 g / 10 min.
[0040] (2) Preparation of B1 layer material: It is obtained by copolymerization of three monomers: terephthalic acid, adipic acid and 1,2,4-butanetriol. The preparation method includes the following steps:
[0041] Terephthalic acid (0.5 mol), adipic acid (0.5 mol), 1,2,4-butanetriol (1.3 mol) and catalyst I (tetrabutyl titanate) were added to a 250 mL four-necked round-bottom flask. The amount of catalyst I was 1.5 mmol, and then the system was evacuated and replaced with nitrogen three times. The temperature was gradually raised to 195°C under normal pressure nitrogen atmosphere, and the water fraction was collected. The esterification reaction was judged to be completed when the esterification water output reached 95% or more of the theoretical value.
[0042] Continue to add catalyst II (tetrabutyl titanate) to the reaction bottle, the amount of catalyst II is 4mmol, gradually reduce the pressure and increase the temperature, evacuate to below 200Pa, increase the temperature to 215℃, carry out polycondensation and dealcoholization reaction, the reaction lasts for 2.5h, then fill the reactor with N2 to normal pressure to obtain copolymer adhesive resin B1, the polymer melt is water-cooled, granulated and dried for standby use. The number average molecular weight M of copolyester B1 n It is 23970 g / mol and PDI is 1.75.
[0043] (3) Preparation of C1 layer material: PVA, white carbon black, and hydrotalcite (1250 mesh) were placed in a high-speed mixer according to the measured components, mixed evenly, and then heated to 80° C., continued to stir, and slowly added glycerol. After the addition was completed, stirring was continued for 10 minutes, and then the material was discharged and extruded and granulated by a twin-screw extruder to obtain a thermoplastic polyvinyl alcohol material. The mass ratio of PVA, white carbon black, hydrotalcite and glycerol was 100:0.3:0.3:25.
[0044] (4) The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded material is blown through the mold to form a five-layer co-extrusion blown film, and the pulling speed after co-extrusion is 2m / min. The total thickness of the five-layer co-extruded high barrier film 1 (A1B1C1B1A1) is 50μm, the single layer thickness of the A1 layer is 10μm, the single layer thickness of the B1 layer is 10μm, and the thickness of the C1 layer is 10μm.
[0045] Example 2
[0046] This embodiment provides a five-layer co-extruded biodegradable barrier film 2, and the preparation method thereof is as follows:
[0047] (1) Preparation of A2 layer materials: The mass ratio of PBAT, PLA and montmorillonite is 16:4:1, and the melt index of the composite material is 4 g / 10 min.
[0048] (2) Preparation of B2 layer material: It is obtained by copolymerizing terephthalic acid, adipic acid and pentane-1,2,5-triol. Other conditions are the same as those in Example 1. The obtained copolymer adhesive resin B2 has a molecular weight of 24600 g / mol and a molecular weight distribution PDI of 1.77.
[0049] (3) Preparation of C2 layer materials: The mass ratio of PVA, white carbon black, hydrotalcite and glycerol is 100:1:0.3:25, and the other steps are the same as in Example 1.
[0050] (4) The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded materials are blown through the mold to form a five-layer co-extrusion blown film, and the pulling speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 2 (A2B2C2B2A2) is 50μm, the single layer thickness of the A2 layer is 10μm, the single layer thickness of the B2 layer is 5μm, and the thickness of the C2 layer is 20μm.
[0051] Example 3
[0052] This embodiment provides a five-layer co-extruded high barrier film 3, and the preparation method thereof is as follows:
[0053] (1) Preparation of A3 layer materials: The mass ratio of PBAT, PBS and montmorillonite is 4:1:1, and the melt index of the composite material is 2 g / 10 min.
[0054] (2) Preparation of B3 layer material: It is obtained by copolymerizing terephthalic acid, adipic acid and 1,2,6-hexanetriol. Other conditions are the same as those in Example 1. The copolymerized adhesive resin B3 is obtained. The molecular weight is 25810 g / mol and the molecular weight distribution PDI is 1.80.
[0055] (3) Preparation of C3 layer materials: The mass ratio of PVA, white carbon black, hydrotalcite and glycerol is 100:1:1:25, and the other steps are the same as in Example 1.
[0056] (4) The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded material is blown through the mold to form a five-layer co-extrusion blown film, and the pulling speed after co-extrusion is 7.5m / min. The total thickness of the five-layer co-extruded high barrier film 3 (A3B3C3B3A3) is 50μm, the single layer thickness of the A3 layer is 10μm, the single layer thickness of the B3 layer is 5μm, and the thickness of the C3 layer is 20μm.
[0057] Example 4
[0058] This embodiment provides a five-layer co-extruded high barrier film 4, and the preparation method thereof is as follows:
[0059] (1) Preparation of A4 layer material: The mass ratio of PBAT to mica is 5:1, and the melt index of the composite material is 2 g / 10 min.
[0060] (2) Preparation of B4 layer material: It is obtained by copolymerization of terephthalic acid, adipic acid and heptane-1,2,7-triol. Catalyst I is titanium ethylene glycol in an amount of 1 mmol. Other conditions are the same as those in Example 1. The obtained copolymer adhesive resin B4 has a molecular weight of 27982 g / mol and a molecular weight distribution PDI of 1.70.
[0061] (3) Preparation of C4 layer materials: The mass ratio of PVA, white carbon black, hydrotalcite and glycerol is 100:2:1:25, and the other steps are the same as in Example 1.
[0062] (4) The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded material is blown through the mold to form a five-layer co-extrusion blown film, and the pulling speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 4 (A4B4C4B4A4) is 50μm, the single layer thickness of the A4 layer is 7.5μm, the single layer thickness of the B4 layer is 15μm, and the thickness of the C4 layer is 5μm.
[0063] Example 5
[0064] This embodiment provides a five-layer co-extruded high barrier film 5, the specific components and preparation method of which are as follows:
[0065] (1) Preparation of A5 layer material: The mass ratio of PBAT to mica is 5:2, and the melt index of the composite material is 1 g / 10 min.
[0066] (2) Preparation of B5 layer material: It is obtained by copolymerizing three monomers: terephthalic acid, adipic acid and octane-1,2,8-triol. Other conditions are the same as those in Example 1 to obtain a copolymer adhesive resin B5 with a molecular weight of 28020 g / mol and a molecular weight distribution PDI of 1.81.
[0067] (3) Preparation of C5 layer materials: The mass ratio of PVA, white carbon black, hydrotalcite and glycerol is 100:2:2:25, and the other steps are the same as in Example 1.
[0068] (4) The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded material is blown through the mold to form a five-layer co-extrusion blown film, and the pulling speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 5 (A5B5C5B5A5) is 50μm, the single layer thickness of the A5 layer is 7.5μm, the single layer thickness of the B5 layer is 10μm, and the thickness of the C5 layer is 15μm.
[0069] Example 6
[0070] This embodiment provides a five-layer co-extruded high barrier film 6, and the preparation method thereof is as follows:
[0071] (1) Preparation of A6 layer material: The mass ratio of PBAT to mica is 20:1, and the melt index of the composite material is 4 g / 10 min.
[0072] (2) Preparation of B6 layer material: It is obtained by copolymerization of three monomers: terephthalic acid, adipic acid and nonane-1,2,9-triol. The molar ratio of nonane-1,2,9-triol to total acid (terephthalic acid and adipic acid) is 1.5:1. Catalyst II is a tetrabutyl titanate / trimethyl phosphate composite system. The molar ratio of tetrabutyl titanate / trimethyl phosphate in the composite system is 1:1. Other conditions are the same as those in Example 1. The obtained copolymer adhesive resin B6 has a molecular weight of 27652 g / mol and a molecular weight distribution PDI of 1.80.
[0073] (3) Preparation of C6 layer materials: The mass ratio of PVA, white carbon black, hydrotalcite and glycerol is 100:1:1:25, and the other steps are the same as in Example 1.
[0074] (4) The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded materials are blown through the mold to form a five-layer co-extrusion blown film, and the pulling speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 6 (A6B6C6B6A6) is 50μm, the single layer thickness of the A6 layer is 10μm, the single layer thickness of the B6 layer is 10μm, and the thickness of the C6 layer is 10μm.
[0075] Example 7
[0076] This embodiment provides a five-layer co-extruded biodegradable barrier film 7, and the preparation method thereof is as follows:
[0077] The difference from Example 1 is that the material preparation of A7 layer is different: the mass ratio of PLA to montmorillonite is 20:1, and the melt index of the composite material is 5 g / 10 min.
[0078] The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180℃, the extrusion temperature of the B layer is 180℃, the extrusion temperature of the C layer is 185℃, and the head mold temperature is 175℃. The extruded materials are blown through the mold to form a five-layer co-extrusion blown film, and the traction speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 7 (A7B7C7B7A7) is 50μm, the single layer thickness of the A7 layer is 10μm, the single layer thickness of the B7 layer is 5μm, and the thickness of the C7 layer is 20μm.
[0079] Example 8
[0080] The difference from Example 1 is that the material preparation of A8 layer is different: the mass ratio of PBS to montmorillonite is 20:1, and the melting index of the composite material is 4 g / 10 min.
[0081] The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded material is blown through the mold to form a five-layer co-extrusion blown film, and the traction speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 8 (A8B8C8B8A8) is 50μm, the single layer thickness of the A8 layer is 10μm, the single layer thickness of the B8 layer is 5μm, and the thickness of the C8 layer is 20μm.
[0082] Example 9
[0083] The difference from Example 1 is that the material preparation of A9 layer is different: the mass ratio of PPC to montmorillonite is 20:1, and the melt index of the composite material is 4 g / 10 min.
[0084] The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded materials are blown through the mold to form a five-layer co-extrusion blown film, and the traction speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 9 (A9B9C9B9A9) is 50μm, the single layer thickness of the A9 layer is 10μm, the single layer thickness of the B9 layer is 5μm, and the thickness of the C9 layer is 20μm.
[0085] Example 10
[0086] The difference from Example 1 is that the material preparation of A9 layer is different: the mass ratio of PBST to montmorillonite is 20:1, and the melt index of the composite material is 5 g / 10 min.
[0087] The A layer, B layer and C layer materials are transported to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 180°C, the extrusion temperature of the B layer is 180°C, the extrusion temperature of the C layer is 185°C, and the head mold temperature is 175°C. The extruded materials are blown through the mold to form a five-layer co-extrusion blown film, and the traction speed after co-extrusion is 4m / min. The total thickness of the five-layer co-extruded high barrier film 10 (A10B10C10B10A10) is 50μm, the single layer thickness of the A10 layer is 10μm, the single layer thickness of the B10 layer is 5μm, and the thickness of the C10 layer is 20μm.
[0088] Embodiment 11
[0089] The difference from Example 1 is:
[0090] The preparation method of the B11 layer material is different. The amount of catalyst I is 0.1% (1 mmol) of the molar amount of the total acid, the molar ratio of the triol to the total acid is 1.1:1, and the temperature is gradually raised to 180°C under normal pressure and inert atmosphere. The amount of catalyst II is 0.35% of the molar amount of the total acid, and the pressure is gradually reduced and the temperature is raised. The vacuum is evacuated to below 200 Pa, and the temperature is raised to 200°C for a condensation dealcoholization reaction.
[0091] The A layer, B layer and C layer materials are conveyed to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 175°C, the extrusion temperature of the B layer is 175°C, the extrusion temperature of the C layer is 180°C, and the head mold temperature is 170°C. The extruded materials are blown through the mold to form a five-layer co-extrusion blown film, and the traction speed after co-extrusion is 2m / min. The total thickness of the five-layer co-extruded high barrier film 11 (A11B11C11B11A11) is 50μm, the single layer thickness of the A11 layer is 10μm, the single layer thickness of the B11 layer is 10μm, and the thickness of the C11 layer is 10μm.
[0092] Example 12
[0093] The difference from Example 1 is:
[0094] The preparation method of B12 layer material is different. The amount of catalyst I is 0.25% (2.5 mmol) of the molar amount of the total acid, the molar ratio of triol to total acid is 1.7:1, and the temperature is gradually raised to 180°C ~ 210°C under normal pressure and inert atmosphere. The amount of catalyst II is 0.45% (4.5 mmol) of the molar amount of the total acid, and the pressure is gradually reduced and the temperature is increased. The vacuum is evacuated to below 200 Pa, and the temperature is raised to 230°C for condensation dealcoholization reaction. The reaction lasts for 3 hours.
[0095] The preparation method of C12 layer materials is different: the mass ratio of PVA, white carbon black, hydrotalcite and glycerol is 100:2.0:2.0:35.
[0096] The A layer, B layer and C layer materials are conveyed to the ABCBA type five-layer co-extrusion blown film unit. The extrusion temperature of the A layer is 185°C, the extrusion temperature of the B layer is 185°C, the extrusion temperature of the C layer is 190°C, and the head mold temperature is 180°C. The extruded material is blown through the mold to form a five-layer co-extrusion blown film, and the traction speed after co-extrusion is 2m / min. The total thickness of the five-layer co-extruded high barrier film 12 (A12B12C12B12A12) is 50μm, the single layer thickness of the A12 layer is 10μm, the single layer thickness of the B12 layer is 10μm, and the thickness of the C12 layer is 10μm.
[0097] Comparative Example 1
[0098] PBAT was used as a bonding layer B to be compounded with the A layer and the C layer, and the remaining steps were the same as in Example 1 to obtain a PBAT / PVA five-layer co-extruded composite film.
[0099] Comparative Example 2
[0100] Commercially available EVA was used as a bonding layer B to be compounded with the A layer and the C layer, and the remaining steps were the same as in Example 1 to obtain a PBAT / PVA five-layer co-extruded composite film.
[0101] Comparative Example 3
[0102] Commercially available EAA was used as a bonding layer B to be compounded with the A layer and the C layer, and the remaining steps were the same as in Example 1 to obtain a PBAT / PVA five-layer co-extruded composite film.
[0103] Five-layer co-extruded film bonding performance test:
[0104] The PBAT / PVA composite film was cut into a size of 15 mm in width and 200 mm in length, and a 180° peel strength test was performed using a universal electronic testing machine at a peeling speed of 300 mm / min.
[0105] Barrier performance test of five-layer co-extruded film:
[0106] Test method and national standard: The water vapor permeability coefficient is tested according to the national standard GB / T 1037-2021, and the test conditions are 38°C and RH90 / 10; the oxygen permeability coefficient is tested according to the national standard GB / T 19789-2021, and the test conditions are 23°C and RH0; the carbon dioxide permeability coefficient is tested according to the national standard GB / T 1038-2000, and the test conditions are 23°C and RH0.
[0107] Performance analysis of five-layer co-extruded biodegradable barrier film:
[0108] Table 1 High barrier film peeling performance test results
[0109]
[0110]
[0111] Table 2 Test results of five-layer co-extruded film properties
[0112]
[0113]
[0114] Table 3 Barrier performance test results of five-layer co-extruded films
[0115]
[0116]
[0117] From the data in Tables 1-3, it can be seen that the peeling force of the five-layer co-extruded biodegradable barrier film produced by the formula of Example 1-12 has a value of about 30N for layer A and layer C, which is higher than the values of no adhesive layer and the common adhesive layer on the market in Comparative Examples 1-3. At the same time, there is no stratification after stretching, and the water vapor permeability, oxygen permeability and carbon dioxide permeability all maintain high barrier performance. It can be seen from Examples 4 and 5 that appropriate thinning of the B layer material is beneficial to the improvement of the gas barrier performance of the film. At the same time, it can be seen from Examples 1, 2 and 3 that the traction speed during blow molding has a significant effect on the gas barrier performance of the film. The greater the traction speed, the better the barrier performance of the film. From the results of the above examples 1-12 and comparative examples 1-3, it can be seen that the "PBAT-PVAlike" adhesive layer resin prepared by the present invention has excellent bonding properties with the A layer containing ester-based structures PBAT, PLA, PBS, PPC, PBST and the C layer of PVA; at the same time, by changing the carbon chain length of the triol monomer required for synthesizing polyester and the molecular weight and distribution of the copolymer, bonding resins with different bonding properties can be prepared. In addition, it can be seen from Example 9 that the difference in the barrier properties of the selected A layer material can directly affect the final barrier properties of the five-layer co-extruded film, providing ideas for the customized preparation of barrier films in the later stage. The films prepared in the above examples meet the actual requirements for biodegradable barrier packaging and can be vigorously promoted and applied.
[0118] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A biodegradable fat-aromatic copolyester based on PBAT-PVA, characterized in that: The structural formula is shown in formula (I): Formula (I) In formula (I), 2≤m≤7, 1:1≤x:y≤1:1.3, and the number average molecular weight is 23000~28100 g / mol.
2. The biodegradable aliphatic-aromatic copolyester according to claim 1, characterized in that: The number average molecular weight is 23970~28020 g / mol, and the molecular weight distribution PDI is 1.70~1.
81.
3. The method for preparing the biodegradable aliphatic-aromatic copolyester based on PBAT-PVA according to claim 1, characterized in that: The steps include: S1, atmospheric pressure esterification reaction: terephthalic acid, adipic acid, triol and catalyst I are added to a reaction vessel, the sum of the molar amounts of terephthalic acid and adipic acid is taken as the molar amount of the total acid, the amount of catalyst I is 0.1%-0.25% of the molar amount of the total acid, the molar ratio of triol to total acid is 1.1:1-1.7:1, the molar ratio of terephthalic acid to adipic acid is 1:1, the temperature is gradually raised to 180°C-210°C under atmospheric pressure and inert atmosphere, the water fraction is collected, and the esterification reaction is judged to be completed when the esterification water output reaches 95% or more of the theoretical value, and the triol is 1,2,4-butanetriol, pentane-1,2,5-triol, 1,2,6-hexanetriol, heptane-1,2,7-triol, octane-1,2,8-triol or nonane-1,2,9-triol; S2. Vacuum polycondensation reaction: Add catalyst II to the reaction vessel in an amount of 0.35%-0.45% of the molar amount of the total acid, gradually reduce the pressure and increase the temperature, evacuate to below 200 Pa, increase the temperature to 200°C-230°C, and carry out polycondensation dealcoholization reaction. The entire polycondensation reaction lasts for 2.5-3 h, and then the reactor is filled with N2 to normal pressure to obtain the target product.
4. The preparation method according to claim 3, characterized in that: The catalyst I described in step S1 is tetrabutyl titanate or titanium ethylene glycol; the catalyst II described in step S2 is tetrabutyl titanate, titanium ethylene glycol or tetrabutyl titanate / trimethyl phosphate.
5. Use of the PBAT-PVA-based biodegradable fat-aromatic copolyester according to claim 1 or the PBAT-PVA-based biodegradable fat-aromatic copolyester obtained by the preparation method according to claim 3 in bonding composite films.
6. A five-layer co-extruded biodegradable barrier film, characterized in that: The five-layer co-extruded biodegradable barrier film is composed of ABCBA layers; the A layer is a modified biodegradable material, the C layer is a high oxygen barrier PVA material, and the B layer is the PBAT-PVA-based biodegradable fat-aromatic copolyester described in claim 1 or the PBAT-PVA-based biodegradable fat-aromatic copolyester obtained by the preparation method described in claim 3. The total thickness of the B layer is 10%-30% of the total thickness of the five-layer co-extruded high barrier film.
7. The five-layer co-extruded biodegradable barrier film according to claim 6, characterized in that: The modified biodegradable material is obtained by filling a barrier filler in a base resin, the base resin is selected from one or more of PBAT, PLA, PBS, PPC, and PBST, and the barrier filler is talcum powder, montmorillonite or mica.
8. The five-layer co-extruded biodegradable barrier film according to claim 6, characterized in that: The high oxygen barrier PVA material is prepared by the following steps: PVA, flow regulator, and processing stabilizer are mixed evenly, then the temperature is raised to 70°C-90°C, stirring is continued, and the plasticizer is slowly added. After the addition is completed, stirring is continued for 8-12 minutes, and then the material is discharged, and then extruded and granulated by a twin-screw extruder to obtain the high oxygen barrier PVA material.
9. The method for preparing a five-layer co-extruded biodegradable barrier film according to any one of claims 6 to 8, characterized in that: The biodegradable barrier film is prepared by five-layer co-extrusion blow molding, which specifically includes the following steps: conveying the A layer, B layer and C layer materials to a five-layer co-extrusion film blowing unit, the extrusion temperature of the A layer is 175°C~185°C, the extrusion temperature of the B layer is 175°C~185°C, the extrusion temperature of the C layer is 180°C~190°C, the head mold temperature is 170°C~180°C, the extruded material is blown through the mold to form a five-layer co-extruded biodegradable barrier film, and the traction speed after co-extrusion is 2.0-7.5 m / min.