A kind of water-based anti-etching ink and its preparation method and application

By using the combination of aqueous silicone modified polyurethane resin and additives, the problem of insufficient printing accuracy and adhesion of existing water-based etching inks is solved, and the etching effect of high adhesion and low wastewater is achieved. It is suitable for copper, tinplate, etc. Metal substrates significantly improve the environmental protection and efficiency of etching.

CN118027736BActive Publication Date: 2024-11-15GUANGZHOU DOLPHIN NEW MATERIALS CO LTD
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
CN202311731426.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-11-15
Estimated Expiration
2043-12-15

AI Technical Summary

Technical Problem

The existing aqueous PCB circuit alkaline etch protection inks have shortcomings in printing accuracy and metal adhesion, and they need to use strong alkali solution to remove, resulting in large amount of wastewater and affecting environmental protection.

Method used

Using aqueous silicone modified polyurethane resin as the main component, combined with additives and solvents, ink is prepared by silk-printing etching, which can achieve high adhesion and etching resistance without adding fillers, and can be easily removed by alcohol solvents. , reduce wastewater production.

Benefits of technology

It achieves high adhesion and high printing accuracy on metal substrates such as copper and tinplate. The etching lines are clear, the line width can be less than 50μm, and there is no circuit breaker or sawtooth phenomenon. At the same time, the amount of wastewater to remove the protective coating is significantly reduced. It has green and environmentally friendly characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118027736B_ABST
    Figure CN118027736B_ABST
Patent Text Reader

Abstract

The present invention provides a water-based anti-etching ink and a preparation method and application thereof. The water-based anti-etching ink comprises: a water-based organosilicon-modified polyurethane resin, an additive, a cosolvent and optional water. The water-based etching ink has excellent adhesion on metal substrates such as copper and tinplate. It not only has excellent anti-etching performance, but can also be easily removed by alcohol solvents. The water-based anti-etching ink can be used in etching circuits. The circuit obtained by silk-screen etching with the water-based anti-etching ink has clear lines and high printing precision, and can print circuits of 50 μm and below. The water-based etching ink provided by the present invention does not need to be faded by a strong alkaline solution, generates very little wastewater, and is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuits, and in particular to a water-based anti-etching ink and a preparation method and application thereof. Background Art

[0002] Etching protection ink can be used to protect the parts that do not need to be etched. It is currently widely used in the fields of hardware etching, stainless steel crafts, circuit board etching, etc. According to the curing method, etching ink can be divided into photosensitive etching ink and thermosetting ink. According to the construction method, it can be printed on copper, aluminum, stainless steel and other substrates by spraying, rolling, silk screen printing and other methods. Among them, the silk screen etching method is to print on the surface of the metal substrate by screen printing, and then use etching liquid for etching after drying. After the etching is completed, the etching protection ink will fade. Compared with photosensitive etching ink, silk screen etching ink is simple to ink, and no exposure and development are required. It not only simplifies the etching process, but also because there is no photosensitizer added to the etching ink, it will not react with light, and there is no need to avoid light for inking. With the continuous improvement of screen printing technology and equipment, screen printing is increasingly used in the electronics industry, gradually forming a new field of electronic screen printing.

[0003] Patent CN108165092A discloses a water-based PCB circuit alkaline etching protective ink and a preparation method thereof. The water-based PCB circuit alkaline etching protective ink comprises the following raw materials in parts by weight: 100 parts of water-based connecting material; 30-50 parts of filler; 5-10 parts of deionized water; 1-3 parts of defoaming agent; 1-3 parts of leveling agent; 3-8 parts of water-based color paste. The use method of the water-based PCB circuit alkaline etching protective ink is as follows: a. On the already exposed design circuit stencil, the protective ink is screen-printed on the PCB board by screen printing; b. It is left in a well-ventilated place for a period of time to wait for the protective ink to dry; c. The PCB board enters the assembly line, first passes through the alkaline etching area, and the etching liquid is sprayed on the circuit board through the nozzle. The copper is etched away by the etching liquid in the places not covered by the protective ink, and then passes through the alkaline fading area, and 2% sodium hydroxide solution is sprayed on the PCB board to dissolve and rinse the protective ink. Finally, the PCB circuit board etching process is completed after water washing and drying. The water-based PCB circuit alkaline etching protection ink disclosed in the patent is green and environmentally friendly and has a certain degree of alkali resistance, but it still has problems such as low printing accuracy and insufficient adhesion. In addition, the water-based PCB circuit alkaline etching protection ink disclosed in the patent, like the etching protection ink disclosed in other prior arts, finally needs to be stripped with a strong alkaline solution, resulting in the generation of a large amount of wastewater.

[0004] In summary, developing a water-based anti-etching ink with high printing accuracy, good metal adhesion and low wastewater generation is an urgent problem to be solved in this field. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an aqueous anti-etching ink and a preparation method and application thereof. The aqueous etching ink has excellent adhesion on metal substrates such as copper and tinplate. It not only has excellent anti-etching performance, but can also be easily removed by alcohol solvents. The circuit obtained by silk-screen etching of the aqueous anti-etching ink has clear lines and high printing precision, and can print circuits of 50 μm and below. The aqueous etching ink provided by the present invention does not need to be faded by a strong alkaline solution, generates very little wastewater, and is green and environmentally friendly.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an aqueous anti-etching ink, comprising: an aqueous silicone-modified polyurethane resin, an auxiliary agent, a co-solvent and optionally water.

[0008] The inventors have found that the water-based organosilicon-modified polyurethane resin not only has good adhesion to metal substrates like conventional water-based polyurethane resins, but also has anti-etching performance and removability that conventional water-based polyurethane resins do not have. The protective ink obtained by combining it with other components can achieve good anti-etching effect without adding fillers, and can be easily removed and has good construction effect. When it is applied to circuit etching, it can not only greatly reduce the cost of use, but also greatly reduce the wastewater generated by removing the protective coating.

[0009] Preferably, the aqueous anti-etching ink comprises, by weight percentage: 50-70% aqueous silicone-modified polyurethane resin (for example, 52%, 55%, 57%, 60%, 62%, 65%, 67%, etc.), 2-10% additives, 15-25% co-solvent (for example, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%), and optionally water.

[0010] Preferably, the co-solvent includes one or more of propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol ether acetate, ethylene glycol monobutyl ether, diethylene glycol butyl ether, propylene glycol butyl ether, and dipropylene glycol butyl ether.

[0011] Preferably, the viscosity of the aqueous anti-etching ink is 5000-10000 cps.

[0012] The invention greatly improves the construction effect and circuit printing effect of the water-based anti-etching ink by controlling the added amount of the co-solvent.

[0013] Preferably, the auxiliary agent includes 1-5% slow-drying auxiliary agent in terms of weight percentage.

[0014] Preferably, the slow-drying auxiliary agent includes one or more of ethylene glycol, propylene glycol, butylene glycol, pentaerythritol, and glycerol.

[0015] Preferably, the auxiliary agent includes 1-5% thickener in terms of weight percentage.

[0016] Preferably, the thickener includes one or more of a cellulose thickener, a polyacrylate thickener, a polyurethane thickener, and an associative thickener.

[0017] Preferably, the auxiliary agent includes 0.5-1% wetting agent in terms of weight percentage.

[0018] Preferably, the wetting agent comprises polyether-modified silicone oil.

[0019] The polyether modified silicone oil may be one or more of Silok8022, Silok8000, Silok8002, Silok8008, Silok8009, Silok8010 and Silok8018 produced by Guangzhou Silok High Molecular Polymer Co., Ltd.

[0020] Preferably, the auxiliary agent includes 0.2-0.5% of a leveling agent in terms of weight percentage.

[0021] Preferably, the leveling agent includes one or more of Silok8160, Silok8224, Silok8225, Silok8232 and Silok8233 produced by Guangzhou Silok Polymer Co., Ltd.

[0022] Preferably, based on the solid content of the water-based silicone-modified polyurethane resin, the silicone content in the water-based silicone-modified polyurethane resin is 55-65%; for example, it can be 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, etc.

[0023] Preferably, the waterborne silicone-modified polyurethane resin includes Dolphin 1528T produced by Guangzhou Dolphin New Materials Co., Ltd.

[0024] In a second aspect, the present invention provides a method for preparing the above-mentioned aqueous anti-etching ink, the preparation method comprising the following steps:

[0025] The water-based organosilicon-modified polyurethane resin, the auxiliary agent, the co-solvent and the optional water are uniformly mixed to obtain the water-based anti-etching ink.

[0026] In a third aspect, the present invention provides a use of an aqueous anti-etching ink in etching circuits.

[0027] In a fourth aspect, the present invention provides an application method of a water-based anti-etching ink, comprising the following steps:

[0028] S1. The aqueous anti-etching ink is applied to the substrate by screen printing;

[0029] S2. After the water-based anti-etching ink is dried, etching is performed. After etching, the water-based anti-etching ink is removed using an alcohol solvent to obtain a circuit.

[0030] Specifically, the alcohol solvent may be ethanol.

[0031] Preferably, the substrate comprises an upper layer and a bottom layer from top to bottom, the upper layer is a copper foil layer or an electroplated copper thin layer; the bottom layer is a silicon layer or a glass layer.

[0032] Preferably, the application method further comprises the step of coating the aqueous anti-etching ink on the edge of the bottom layer.

[0033] In a fifth aspect, the present invention provides a circuit board, comprising a circuit prepared by the above method.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention provides a water-based anti-etching ink, which is obtained by using a water-based organosilicon-modified polyurethane resin as a main resin and mixing an auxiliary agent and a cosolvent. The water-based anti-etching ink has good adhesion on a metal substrate, a simple construction process, and a good silk-screen printing effect; after film formation, due to the enrichment of a large number of organosilicon segments on the surface, the ink coating is endowed with excellent anti-etching ability and the effect of being easily removed, and the line width of the circuit obtained by etching can be less than 50 μm, and the lines are clear, without circuit breakage and sawtooth phenomena. The application of the water-based anti-etching ink to circuit etching can not only greatly reduce the use cost, but also greatly reduce the wastewater generated by removing the protective coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a partial image of the etched circuit prepared in Application Example 1 of the present invention under a microscope. DETAILED DESCRIPTION

[0037] The technical scheme of the present invention is further described below by specific embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. In addition, about "parts" and "%" in this specification, unless otherwise specified, represent "parts by mass" and "mass %" respectively.

[0038] In the present invention, the raw material information involved in each embodiment is as follows:

[0039] Water-based silicone-modified polyurethane resin: dolphin1528T produced by Guangzhou Dolphin New Materials Co., Ltd. (based on the total weight of solids of the water-based silicone-modified polyurethane resin, the silicone content accounts for 60wt%).

[0040] 1. Preparation of water-based etching circuit protection ink. Example 1

[0041] A water-based etching circuit protection ink comprises, in 100 parts by weight, 65 parts of water-based silicone modified polyurethane resin, 3 parts of propylene glycol, 0.5 parts of wetting agent (Silok 8022, Guangzhou), 0.5 parts of leveling agent (Silok 8160, Guangzhou), 20 parts of ethylene glycol monobutyl ether, 2 parts of associative thickener (Silok 02, Guangzhou) and the balance of deionized water.

[0042] A method for preparing a water-based anti-etching ink comprises the following steps:

[0043] The water-based silicone modified polyurethane resin, propylene glycol, a wetting agent (Silok8022), a leveling agent (Silok8160), ethylene glycol monobutyl ether and deionized water were mixed, stirred at 600 rpm for 20 minutes, and then an associative thickener (Silok02) was added for thickening. After vacuum defoaming, the mixture was filtered and packaged to obtain a water-based anti-etching ink. Example 2

[0044] A water-based etching circuit protection ink comprises, in 100 parts by weight, 50 parts of water-based silicone modified polyurethane resin, 5 parts of butanediol, 0.5 parts of wetting agent (Silok 8022, Guangzhou), 0.2 parts of leveling agent (Silok 8160, Guangzhou), 15 parts of ethylene glycol monobutyl ether, 5 parts of associative thickener (Silok 02, Guangzhou) and the balance of deionized water.

[0045] A method for preparing a water-based anti-etching ink comprises the following steps:

[0046] The water-based silicone modified polyurethane resin, butanediol, a wetting agent (Silok8022), a leveling agent (Silok8160), ethylene glycol monobutyl ether and deionized water were mixed, stirred at 400 rpm for 20 minutes, and then an associative thickener (Silok02) was added for thickening. After vacuum defoaming, the mixture was filtered and packaged to obtain a water-based anti-etching ink. Example 3

[0047] A water-based etching circuit protection ink comprises, based on 100 parts by weight, 70 parts of water-based silicone modified polyurethane resin, 2 parts of ethylene glycol, 1 part of wetting agent (Silok 8022, Guangzhou), 0.5 parts of leveling agent (Silok 8160, Guangzhou), 25 parts of ethylene glycol monobutyl ether, 1 part of associative thickener (Silok 02, Guangzhou) and the balance of deionized water.

[0048] A method for preparing a water-based anti-etching ink comprises the following steps:

[0049] The water-based silicone modified polyurethane resin, ethylene glycol, a wetting agent (Silok8022), a leveling agent (Silok8160), ethylene glycol monobutyl ether and deionized water were mixed, stirred at 400 rpm for 20 minutes, and then an associative thickener (Silok02) was added for thickening. After vacuum defoaming, the mixture was filtered and packaged to obtain a water-based anti-etching ink. Example 4

[0050] The difference between this embodiment and embodiment 1 is that:

[0051] While keeping the weight of the water-based etching circuit protection ink unchanged at 100 parts by weight, 10 parts by weight of ethylene glycol monobutyl ether are added in this embodiment, and 10 parts by weight of deionized water are correspondingly added.

[0052] The aqueous anti-etching ink was prepared by the same preparation method as in Example 1. Example 5

[0053] The difference between this embodiment and embodiment 1 is that:

[0054] While keeping the weight of the water-based etching circuit protection ink unchanged at 100 parts by weight, 30 parts by weight of ethylene glycol monobutyl ether are added in this embodiment, and the weight of deionized water is correspondingly reduced by 10 parts by weight.

[0055] The aqueous anti-etching ink was prepared by the same preparation method as in Example 1.

[0056] Comparative Example 1

[0057] The difference between this comparative example and Example 1 is that this comparative example uses a water-based polyurethane resin (Lubrizol Sancure 2710; the silicone content is 0 wt %).

[0058] Comparative Example 2

[0059] The difference between this comparative example and Example 1 is that: while keeping 100 parts by weight of the water-based etching circuit protection ink unchanged, no co-solvent is added in this comparative example, and 20 parts by weight of deionized water is correspondingly increased.

[0060] Application Examples 1~5, Comparative Application Examples 1~2

[0061] A method for preparing an etching circuit, comprising:

[0062] (1) A wafer with a copper foil layer is used as a substrate;

[0063] (2) Screen printing the water-based anti-etching ink (Examples 1-5, Comparative Examples 1-2) on the surface of the copper foil layer through a 325-mesh screen; and coating the edge of the wafer with the above-mentioned water-based anti-etching ink as protection; and baking at 90° C. for 1 min;

[0064] (3) The dried protective ink layer is etched with an alkaline etching solution. After the etching is completed, the aqueous anti-etching ink is wiped off with ethanol to obtain the etched circuit.

[0065] Test Example 1

[0066] The water-based anti-etching ink obtained in Examples 1 to 5 and Comparative Example 1 was diluted to 20 seconds (four cups of coating) and sprayed on tinplate respectively. After drying at 120° C. for 2 hours, a test sample was obtained and tested according to the following method. The test results are shown in Table 1.

[0067] (1) Adhesion: GB / T9286-1998 "Scratch test for paint and varnish films", where grade 0 is the best and grade 5 is the worst.

[0068] (2) Alkaline etching resistance: The above test sample was immersed in an alkaline etching solution of ammonium chloride and ammonia water at a temperature of 45°C. After immersion for 1 min, it was taken out, washed with clean water and blown dry, and then the adhesion was tested according to the method of standard GB / T9286-1998.

[0069] Table 1

[0070]

[0071] It can be seen from Table 1 that the water-based anti-etching ink obtained in the embodiment of the present invention has good adhesion and alkaline etching resistance on the metal substrate.

[0072] From the comparison between Example 1, Example 4 and Example 5, it can be seen that too high or too low an amount of the solvent added will affect the adhesion and alkaline etching resistance of the coating.

[0073] From the comparison between Example 1 and Comparative Example 1, it can be seen that when the water-based anti-etching ink uses a polyurethane resin without silicone segments as a film-forming resin and is used in a relatively high amount of a solvent, the adhesion and alkaline etching resistance of the resulting coated metal are not as good as those of the water-based anti-etching ink obtained in Example 1.

[0074] Test Example 2

[0075] The circuits obtained from the above-mentioned application examples 1 to 5 and the application comparison examples 1 to 2 were evaluated according to the following method. The evaluation results are shown in Table 2.

[0076] (1) Etching effect: Observe the circuit under a microscope and magnify it 1000 times to see whether the circuit has clear lines, any broken circuits, or obvious jagged edges. If the lines are clear, and there are no broken circuits or obvious jagged edges, the circuit is qualified; otherwise, it is unqualified.

[0077] (2) Film removal effect: Observe whether there is any residual protective ink coating on the surface of the substrate after film removal. If the film is removed cleanly without any residue, it is qualified, otherwise it is unqualified.

[0078] Table 2

[0079]

[0080] From Table 1 and Table 2 and Figure 1 It can be seen that the adhesion of the water-based anti-etching ink provided in the embodiments of the present invention on the metal is all level 0, and it still has excellent adhesion after being treated with the etching solution. It can be seen that the water-based anti-etching ink of the present invention not only has excellent adhesion but also has excellent alkaline etching resistance. The line width of the circuit obtained by etching can be less than 50μm, and the lines are clear without disconnection and sawtooth phenomenon.

[0081] From the comparison between Comparative Example 1 and Example 1, it can be seen that when Comparative Example 1 uses a water-based polyurethane resin without silicone as a film-forming resin, the anti-etching ability and etching effect of the obtained water-based anti-etching ink are significantly reduced.

[0082] From the comparison between comparative application example 2 and application example 1, it can be seen that in comparative application example 2, no solvent is added, and the circuit effect obtained by etching is worse.

[0083] The present invention uses the above embodiments to illustrate a water-based anti-etching ink and its preparation method and application, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A water-based anti-etching ink, characterized in that: The water-based anti-etching ink comprises, by weight percentage, 50-70% water-based silicone-modified polyurethane resin, 2-10% additive, 16-25% cosolvent, and water; The organic silicon content in the aqueous organic silicon modified polyurethane resin is 55-65% based on the solid content of the aqueous organic silicon modified polyurethane resin.

2. The water-based anti-etching ink according to claim 1, characterized in that: The viscosity of the aqueous anti-etching ink is 5000-10000 cps.

3. The water-based anti-etching ink according to claim 1, characterized in that: According to weight percentage, the auxiliary agent includes 1-5% slow-drying auxiliary agent.

4. The water-based anti-etching ink according to claim 1, characterized in that: According to weight percentage, the auxiliary agent includes 1-5% thickener.

5. The water-based anti-etching ink according to claim 1, characterized in that: According to weight percentage, the auxiliary agent includes 0.5-1% wetting agent.

6. The water-based anti-etching ink according to claim 1, characterized in that: According to weight percentage, the auxiliary agent includes 0.2-0.5% leveling agent.

7. The water-based anti-etching ink according to claim 1, characterized in that: The waterborne silicone-modified polyurethane resin includes Dolphin 1528T.

8. A method for preparing the water-based anti-etching ink according to any one of claims 1 to 7, characterized in that: The steps include: The water-based organosilicon-modified polyurethane resin, the auxiliary agent, the cosolvent and water are uniformly mixed to obtain the water-based anti-etching ink.

9. Use of the aqueous anti-etching ink according to any one of claims 1 to 8 in etching circuits.

10. A method for applying a water-based anti-etching ink, characterized in that: The steps include: S1. Applying the aqueous anti-etching ink according to any one of claims 1 to 7 on a substrate by screen printing; S2. After the water-based anti-etching ink is dried, etching is performed. After etching, the water-based anti-etching ink is removed using an alcohol solvent to obtain a circuit.

11. The application method according to claim 10, characterized in that: The substrate comprises an upper layer and a bottom layer from top to bottom, wherein the upper layer is a copper foil layer or an electroplated copper thin layer; and the bottom layer is a silicon layer or a glass layer.

12. The application method according to claim 11, characterized in that: The method further comprises the step of coating the aqueous anti-etching ink on the edge of the bottom layer.

13. A circuit board, characterized in that: The invention comprises a circuit prepared by the method described in any one of claims 10 to 12.

Citation Information

Patent Citations

  • Aqueous PCB circuit alkaline etching protective printing ink and preparation method thereof

    CN108165092A

  • Ultraviolet curing organic silicon modified polyurethane aqueous dispersoid and preparation method thereof

    CN101735599A

  • Etching-resistant composition and application thereof

    CN102786838A

  • Waterproof and light-resistant water-based resin dye jet ink

    CN103087586A

  • Water-based pigment ink for quality improvement

    CN103319953A