Al-Si aluminum alloy and preparation method thereof, and heat dissipation structure
By adding specific elements to Al-Si aluminum alloys and refining and aging treatment, excellent mechanical and thermal conductivity are formed, and the existing aluminum alloy molding performance and cost control problems are solved, and aluminum alloys are realized in the electronic information industry. Widely used.
Patent Information
- Application Number
- CN202410168149.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-02-05
AI Technical Summary
While improving thermal conductivity and mechanical properties of existing aluminum alloys, it is difficult to take into account both molding performance and cost control. In particular, aluminum alloys with high thermal conductivity are relatively high and have poor molding properties, which affects their wide application in the electronic information industry.
Developed an Al-Si aluminum alloy containing specific ranges of Si, Fe, Cu, Mg, Sr, Zn, Ni, B and other elements. Through refining and aging treatment, excellent mechanical properties, thermal conductivity and molding properties are formed. And reduce the solid solubility through elemental interactions and increase the volume fraction of the precipitated phase.
It achieves the high thermal conductivity, excellent mechanical properties and good molding properties of aluminum alloys, reduces the adverse impact of alloy elements on thermal conductivity, improves the comprehensive performance of aluminum alloys, and is suitable for the heat dissipation structure of the electronic information industry.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to an Al-Si series aluminum alloy, a preparation method of the Al-Si series aluminum alloy, and a heat dissipation structure. Background Art
[0002] With the rapid development of the new generation of electronic information technology, the high efficiency and rapid operation, high integration, and miniaturization of related equipment have become a trend. Communication base station heat dissipation housings, computer equipment heat sinks, mobile phone mid-plates, etc. have put forward higher requirements for heat dissipation performance. Therefore, it is very necessary to develop new materials with high thermal conductivity and easy molding to improve the heat dissipation capacity of devices or equipment.
[0003] Aluminum alloy has good comprehensive properties, with advantages such as high strength, low density, good electrical and thermal conductivity, and easy processing and cutting. The research on high thermal conductivity aluminum alloy is mainly focused on deformed aluminum alloy and its composite materials, but the cost of deformed aluminum alloy and its composite materials is high and the formability is poor. Although the thermal conductivity of die-cast aluminum alloy is low, it has the advantages of good fluidity, easy forming and processing, and low cost. Therefore, die-cast aluminum alloy is currently the most widely used in the electronic information industry.
[0004] Die-cast aluminum alloys mainly include aluminum-silicon die-cast aluminum alloys and aluminum-magnesium die-cast aluminum alloys. In aluminum-silicon die-cast aluminum alloys, as the silicon content increases, the fluidity and density of the alloy gradually improve, and the forming performance and mechanical properties are better, which can be widely used in heat dissipation parts. However, the addition of silicon does not improve the mechanical properties much. In order to ensure excellent mechanical properties, other alloying elements must be added. However, the thermal conductivity of aluminum alloys is affected by the scattering of free electrons in the crystal. The addition of alloying elements will inevitably affect the uniformity and purity of the aluminum matrix, which will hinder the thermal conductivity of aluminum alloys. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the present invention provides an Al-Si series aluminum alloy, aiming to obtain an Al-Si series aluminum alloy with excellent thermal conductivity, mechanical properties, and die-casting properties.
[0006] The present invention provides an Al-Si aluminum alloy, which contains aluminum, 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass.
[0007] Furthermore, the Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.05% Zn by mass, 0.01-0.09% Ni by mass, 0.0009-0.01% B by mass, 0.001-0.008% Mn by mass, 0.001-0.008% Ti by mass, 0.001-0.008% Cr by mass, and 0.001-0.008% V by mass.
[0008] Furthermore, at least one of the following conditions is met:
[0009] The mass ratio of Si to Fe is 5-20:1;
[0010] The mass ratio of Si to Sr is 200-1500:1;
[0011] The mass ratio of Mg, Cu, and Zn is 0.1-1:0.1-1:1;
[0012] The sum of the mass percentages of Cu, Mg, Zn, and B shall not exceed 0.2%;
[0013] The sum of the mass percentages of Si, Fe, Cu, Mg, Sr, Zn, Ni, and B shall not exceed 9%;
[0014] The Al-Si aluminum alloy further contains Mn, Ti, Cr, and V, and the sum of the mass percentages of Mn, Ti, Cr, and V is not greater than 0.03%;
[0015] The mass percentage content of a single impurity in the Al-Si aluminum alloy is less than 0.02%, and the sum of the mass percentage content of the impurities is less than 0.1%.
[0016] Furthermore, at least one of the following conditions is met:
[0017] The Al-Si aluminum alloy further contains 0-0.009% by mass of In;
[0018] The Al-Si aluminum alloy further contains 0-0.005% by mass of Nb;
[0019] The Al-Si aluminum alloy further contains Bi in an amount of 0-0.006% by mass;
[0020] The Al-Si aluminum alloy further contains Ge in an amount of 0-0.005% by mass;
[0021] The Al-Si aluminum alloy further contains 0-0.005% by mass of Mo;
[0022] The Al-Si aluminum alloy also contains Ag in an amount of 0-0.005% by mass;
[0023] The Al-Si aluminum alloy further contains Sn in an amount of 0-0.1% by mass;
[0024] The Al-Si aluminum alloy also contains Te in an amount of 0-0.005% by mass;
[0025] The Al-Si aluminum alloy further contains 0-0.01% Be by mass;
[0026] The Al-Si aluminum alloy further contains Co in an amount of 0-0.1% by mass;
[0027] The Al-Si aluminum alloy also contains Cd in an amount of 0-0.01% by mass;
[0028] The Al-Si aluminum alloy further contains RE in an amount of 0-0.02% by mass, wherein RE is at least one of La, Ce, Pr, Nd, Er, Sm, Y, and Gd.
[0029] Furthermore, at least one of the following conditions is met:
[0030] When the Al-Si aluminum alloy contains In, the mass ratio of Cu to In is 0.1-20:1;
[0031] When the Al-Si aluminum alloy contains Nb, the mass ratio of Ni to Nb is 1-50:1;
[0032] When the Al-Si aluminum alloy contains Bi, the mass ratio of Mg to Bi is 10-450:1;
[0033] When the Al-Si aluminum alloy contains Ge, the mass ratio of Si to Ge is 1000-2000:1;
[0034] When the Al-Si aluminum alloy contains Mo, the mass ratio of Si to Mo is 1500-2000:1;
[0035] When the Al-Si aluminum alloy contains Ag, the mass ratio of Mg to Ag is 10-500:1, and the mass ratio of Cu to Ag is 10-400:1;
[0036] When the Al-Si aluminum alloy contains Sn and Te, the mass ratio of Mg to Sn is 0.3-10:1, and the mass ratio of Te to Sn is 0.01-1:1;
[0037] When the Al-Si aluminum alloy contains Be and Co, the mass ratio of Be, Co, and Fe is 0.001-0.03:0.004-0.25:1, and the mass ratio of Fe and Co is 1-250:1;
[0038] When the Al-Si aluminum alloy contains RE, Be, and Cd, the mass ratio of RE, Sr, and Fe is 0.002-0.1:0.02-0.08:1, the mass ratio of RE, B, and Fe is 0.002-0.1:0.0001-0.03:1, the mass ratio of RE and Cd is 0.1-25:1, and the mass ratio of RE, B, and Be is 0.5-20:0.1-10:1.
[0039] Furthermore, the Al-Si aluminum alloy further contains 0.0001-0.009% by mass of In, 0.0001-0.005% by mass of Nb, 0.0001-0.006% by mass of Bi, 0.0001-0.005% by mass of Ge, 0.0001-0.005% by mass of Mo, and 0.0 0.001-0.005% Ag, 0.0001-0.1% Sn, 0.0001-0.005% Te, 0.0001-0.01% Be, 0.001-0.1% Co, 0.001-0.008% Cd, and 0.001-0.02% RE.
[0040] The present invention also provides a method for preparing an Al-Si series aluminum alloy, comprising the following steps:
[0041] The aluminum source is subjected to a first heating treatment to obtain aluminum liquid;
[0042] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and B to the aluminum liquid, performing a second heating treatment, and obtaining an alloy liquid;
[0043] Refining and slagging the alloy liquid, and testing its composition and content;
[0044] After the composition and content are qualified, the alloy liquid after the refining treatment and the slag removal treatment is subjected to die casting treatment and aging treatment to obtain an Al-Si series aluminum alloy, wherein the Al-Si series aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass.
[0045] Further, the aging treatment temperature is 280° C. to 350° C., and the time is 0.05 h to 15 h; or
[0046] The aging treatment includes a primary low-temperature aging treatment, a secondary low-temperature aging treatment, and a tertiary high-temperature aging treatment, wherein the temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1h to 15h; the temperature of the secondary low-temperature aging treatment is 0°C to 70°C, and the time is 1h to 24h; the temperature of the tertiary high-temperature aging treatment is 280°C to 350°C, and the time is 0.05h to 15h.
[0047] Furthermore, at least one of the following conditions is met:
[0048] The aluminum source is at least one of original aluminum, aluminum ingot, and recycled aluminum;
[0049] The preparation method of the Al-Si aluminum alloy also includes the step of adding at least one of In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE to the aluminum liquid.
[0050] The present invention also provides a heat dissipation structure, wherein at least part of the heat dissipation structure is made of the Al-Si series aluminum alloy or the Al-Si series aluminum alloy prepared by the preparation method of the Al-Si series aluminum alloy.
[0051] In the technical solution of the present invention, the Al-Si aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass. Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, and on the basis of ensuring that the Al-Si aluminum alloy has better formability, it also has excellent mechanical properties and thermal conductivity. The details are as follows:
[0052] (1) When the mass percentage of Si is 5-8%, on the one hand, Si can improve the fluidity and density of aluminum alloy, thereby improving the forming performance and mechanical properties of aluminum alloy. On the other hand, Si can react with other elements to form a second phase as much as possible to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of aluminum alloy. Specifically, Si can react with Al, Fe, Cu, Mg, Mn, B, etc. to form Mg 2 Second phases such as Si, AlFeSi, AlMnSi, AlFeSiCu, AlFeMgSi, AlFeSiB, AlFeMnSi;
[0053] (2) When the mass percentage of Fe is 0.4-0.8%, on the one hand, Fe can reduce the sticking tendency of aluminum alloy castings and improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Fe can react with other elements to form a second phase as much as possible to avoid the adverse effect of Fe dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Fe can react with Al, Si, Mg, Cu, Mn, Ni, B, etc. to form Al 3 Fe, AlFeSi, AlFeMgSi, AlFeSiB, AlFeSiCu, AlFeSiNi, AlFeMgSiNi, AlFeMnSi, FeNiAl 9 Wait for the second phase;
[0054] (3) When the mass percentage of Cu is 0.001-0.05%, on the one hand, Cu can improve the mechanical properties, thermal conductivity, and fatigue resistance of aluminum alloys, and on the other hand, Cu can react with other elements as much as possible to form a second phase to avoid the adverse effect of Cu dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Cu can react with Al, Fe, Si, Mg, Zn, etc. to form CuAl 2 、AlFeSiCu、Al 2CuZn, (CuMg)Al 2 In addition, Cu can also promote Mg 2 Si、Mg 2 Zn、Mg 2 SiZn、(CuMg)Al 2 , AlFeMgSi, AlFeMgSiNi and other second phases are precipitated to increase their volume fraction and dispersion degree, so as to reduce the solid solubility of the above elements in the aluminum matrix;
[0055] (4) When the mass percentage of Mg is 0.001-0.05%, on the one hand, Mg can improve the mechanical properties and thermal conductivity of aluminum alloys, and on the other hand, Mg can react with other elements to form a second phase as much as possible to avoid the adverse effect of Mg dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Mg can react with Al, Fe, Si, Cu, Zn, Ni, etc. to form Mg 2 Si、Mg 2 Zn、Mg 2 SiZn、(CuMg)Al 2 , AlFeMgSi, AlFeMgSiNi and other second phases. In addition, Mg can also promote CuAl 2 、AlFeSiCu、Al 2 CuZn, (CuMg)Al 2 The precipitation of the second phase, etc., increases its volume fraction and dispersion, thereby reducing the solid solubility of the above elements in the aluminum matrix;
[0056] (5) When the mass percentage of Sr is 0.005-0.04%, on the one hand, Sr can be modified through the heterogeneous nucleation theory or twin valley mechanism to refine the second phase such as eutectic silicon, improve the thermal conductivity and mechanical properties of the aluminum alloy, and transform the β-AlFeSi phase in the ingot into the Chinese character α-AlFeSi phase to improve the mechanical properties of the aluminum alloy. On the other hand, Sr can preferentially combine with Fe, Cu, Mn, Cr, Si and other elements to form dispersion strengthening to avoid the adverse effect of Sr dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. In addition, Sr can also promote CuAl 2 Mg 2 The precipitation of Si and other phases reduces the solid solubility of these alloy elements in the aluminum matrix;
[0057] (6) When the mass percentage of Zn is 0.001-0.1%, on the one hand, Zn can improve the mechanical properties of aluminum alloys, and on the other hand, Zn can react with other elements to form a second phase as much as possible to avoid the adverse effect of Zn dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Zn can react with Al, Mg, Cu and Si to form MgZn 2 Mg2 SiZn、Al 2 CuZn and other secondary phases. In addition, Zn can eliminate Si to reduce the adverse effects of Si on the performance of aluminum alloys. Zn can also promote Mg 2 Si、Al 2 The precipitation of Cu and other phases improves mechanical properties and thermal conductivity;
[0058] (7) When the mass percentage of Ni is 0.01-0.2%, Ni can be used to improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Ni can be made to react with other elements to form a second phase as much as possible to avoid the adverse effect of Ni dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Ni can react with Al, Fe, Mg, Si, etc. to form Al 3 Ni, AlFeSiNi, AlFeMgSiNi, FeNiAl 9 The second phase promotes the precipitation of elements such as Cu, Mg, Zn, Si, and Fe dissolved in the alloy; Ni can also refine the grains and promote the CuAl 2 、(CuMg)Al 2 Mg 2 The precipitation of strengthening phases such as Si increases the volume fraction and dispersion of the precipitated phase to reduce the solid solubility of alloy elements in the aluminum matrix. In addition, Ni, Cu and Mg can promote each other's precipitation to improve the thermal conductivity and mechanical properties of aluminum alloys.
[0059] (8) When the mass percentage content of B is 0.0008-0.01%, on the one hand, B can react with transition elements Ti, Mn, Cr, V, etc. that sharply reduce the thermal conductivity to form borides. The borides are removed during slagging and sedimentation after the melt is left to stand, thereby reducing the content of Ti, Mn, Cr, and V in the melt. On the other hand, B can also react with other elements to form a second phase as much as possible to avoid the adverse effect of B dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, B can react with Al, Fe, Si, Mn, etc. g, Cu and other reactions generate AlFeSiB, MgB, CuB and other secondary phases, which can not only reduce the solubility of the above elements in the matrix, but also increase the proportion of the precipitated phases of these elements, thereby improving the mechanical properties of the aluminum alloy and the thermal conductivity of the aluminum alloy. In addition, B can also refine the grains, modify and refine the elemental Si to reduce the adverse effects of coarse elemental Si on the performance of the aluminum alloy, and can also transform the β-AlFeSi phase into the Chinese character α-AlFeSi phase to eliminate the adverse effects of the iron-rich phase on the performance of the aluminum alloy, and can inhibit the Ti 3 Segregation of Al.
[0060] Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, which can remove the content of transition elements Ti, Mn, Cr, and V in the aluminum matrix that have a great impact on thermal conductivity, refine the grains, reduce the solid solubility of alloy elements in the aluminum matrix, and increase the volume fraction of the precipitated phase, so as to reduce the adverse effects of alloy elements on the thermal conductivity of aluminum alloys and improve the comprehensive properties of aluminum alloys (including mechanical properties, thermal conductivity, and forming properties, etc.). At the same time, under the further action of aging treatment, the solid solubility of each element in the aluminum matrix is further reduced, which can eliminate the adverse effects of alloy elements on the thermal conductivity of aluminum alloys as much as possible, and the second phase (such as Al 3 Fe、Mg 2 Si、Al 2 Cu, AlFeSiNi, AlMnSi, etc.) can also be refined in the aluminum matrix and at the grain boundaries or within the grain boundaries, greatly improving the mechanical properties and thermal conductivity of the aluminum alloy.
[0061] Specifically, since transition elements such as Mn, Cr, Ti, and V have a great influence on the thermal conductivity and mechanical properties of aluminum alloys, their content needs to be strictly controlled; when the amount of elements such as Cu, Mg, Zn, and B added is large, the thermal conductivity and mechanical properties of the aluminum alloy will also be reduced, and their content also needs to be controlled; but when the mass percentage content of at least one of Cu, Mg, Zn, B, Mn, Cr, Ti, and V is low, the elements with a low mass percentage content are not easy to precipitate, and will exist in the aluminum matrix in the form of solid solution, thereby reducing the thermal conductivity and mechanical properties of the aluminum alloy, and the refinement and modification effect of the aluminum alloy will also deteriorate, causing the single Si at the grain boundary of the aluminum alloy to exist in the form of coarse flakes and strips, seriously splitting the aluminum matrix, and further reducing the thermal conductivity and mechanical properties of the aluminum alloy. In the technical solution of the present invention, as described in the above items (1) to (8), Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, which can refine the grains (such as the modification effect of Sr, the grain refining effect of Ni and B), reduce each other's solid solubility in the aluminum matrix (such as the elements can react with each other to form a second phase), and increase the volume fraction of the precipitated phase (such as Cu, Mg, Sr, Zn, and Ni can promote the precipitation of the second phase), so as to improve the mechanical properties and thermal conductivity of the aluminum alloy; even if the mass percentage content of one or some elements is low, during the aging treatment process, all or almost all of the elements can be precipitated, avoiding adverse effects on the thermal conductivity of the aluminum alloy. DETAILED DESCRIPTION
[0062] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] An embodiment of the present invention provides an Al-Si aluminum alloy, which contains aluminum, and further contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass.
[0064] In a preferred embodiment, the Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.04% Zn by mass, 0.01-0.09% Ni by mass, and 0.0009-0.01% B by mass.
[0065] The sum of the mass percentages of Si, Fe, Cu, Mg, Sr, Zn, Ni, and B is not greater than 9%, preferably not greater than 8.5%, and more preferably not greater than 8%. In this way, while ensuring excellent mechanical properties and thermal conductivity of the aluminum alloy, excessive addition of elements resulting in excessive solid solution in the aluminum matrix is avoided.
[0066] The mass percentage content of Si can be 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, or 8%.
[0067] The mass percentage content of Fe can be 0.4%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%, 0.46%, 0.47%, 0.48%, 0.49%, 0.5%, 0.51%, 0.52%, 0.53%, 0.54%, 0.55%, 0.56%, 0.57%, 0.58%, 0.5 9%, 0.6%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.7%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, or 0.8%.
[0068] The mass percentage content of Cu can be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.02%, 0.021%, 0.022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.030%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.056%, 0.057%, 0.058%, 0.059%, 0.060%, 0. .025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.04%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, or 0.05%.
[0069] The mass percentage content of Mg can be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.02%, 0.021%, 0.022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.030%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.056%, 0.057%, 0.058%, 0.059%, 0.060%, 0. .025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.04%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, or 0.05%.
[0070] The mass percentage content of Sr can be 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.02%, 0.021%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, 0.051%, 0.052%, 0.053%, 0.054%, 0.055%, 0.056%, 0.057%, 0.058%, 0.059%, 0.060%, 0.061%, 0.062%, 0.063%, 0.064%, 0.065%, 0.066%, 0.067%, 0.068%, 0.069%, 0.070%, 0.071%, 0.072%, 0.073%, 0.074%, 0.075%, 0 .022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, or 0.04%.
[0071] The mass percentage content of Zn can be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.012%, 0.014%, 0.016%, 0.018%, 0.02%, 0.022%, 0.024%, 0.026%, 0.028%, 0.03%, 0.032%, 0.034%, 0.036%, 0.038%, 0.04%, 0.042%, 0.0 44%, 0.046%, 0.048%, 0.05%, 0.052%, 0.054%, 0.056%, 0.058%, 0.06%, 0.062%, 0.064%, 0.066%, 0.068%, 0.07%, 0.072%, 0.074%, 0.076%, 0.078%, 0.08%, 0.082%, 0.084%, 0.086%, 0.088%, 0.09%, 0.092%, 0.094%, 0.096%, 0.098%, or 0.1%.
[0072] The mass percentage content of Ni can be 0.01%, 0.012%, 0.014%, 0.016%, 0.018%, 0.02%, 0.022%, 0.024%, 0.026%, 0.028%, 0.03%, 0.032%, 0.034%, 0.036%, 0.038%, 0.04%, 0.042%, 0.044%, 0.046%, 0.048%, 0.05%, 0.052%, 0.054%, 0.056%, 0.058%, 0.06%, 0.06% and 0.0 0.092%, 0.094%, 0.096%, 0.098%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, or 0.2%.
[0073] The mass percentage content of B may be 0.0008%, 0.0009%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, or 0.01%.
[0074] The sum of the mass percentages of Cu, Mg, Zn, and B is no more than 0.2%, preferably 0.15%, and more preferably no more than 0.12%. In one embodiment, the sum of the mass percentages of Cu, Mg, Zn, and B is 0.0038-0.2%, preferably 0.005-0.15%, and more preferably 0.008-0.1%.
[0075] The sum of the mass percentages of Cu, Mg, and Zn is no greater than 0.19%, preferably 0.14%, and more preferably no greater than 0.11%. In one embodiment, the sum of the mass percentages of Cu, Mg, and Zn is 0.003-0.2%, preferably 0.005-0.14%, and more preferably 0.01-0.1%.
[0076] The mass ratio of Si to Fe is 5-20:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Fe is preferably 10-20:1, and more preferably the mass ratio of Si to Fe is 15-20:1, specifically 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, or 20:1.
[0077] The mass ratio of Si to Sr is 200-1500:1. Within the range of this mass ratio, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Sr is preferably 500-1000:1, more preferably 700-800:1, and specifically can be 200:1, 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 550:1, 600:1, 650:1, 700:1, 750:1, 800:1, 850:1, 900:1, 950:1, 1000:1, 1100:1, 1200:1, 1300:1, 1400:1, or 1500:1.
[0078] The mass ratio of Mg, Cu, and Zn is 0.1-1:0.1-1:1. Within this mass ratio range, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg, Cu, and Zn is preferably 0.2-1:0.2-0.8:1, more preferably 0.5-0.8:0.5-0.8:1, specifically 0.1:0.1:1, 0.1:0.2:1, 0.1:0.4:1, 0.1:0.6:1, 0.1:0.8:1, 0.1:1:1, 0.5:0.1:1, 0.5:0.2:1, 0.5:0.4:1, 0.5:0.6:1, 0.5:0.8:1, 0.5:1:1, 1:0.1:1, 1:0.2:1, 1:0.4:1, 1:0.6:1, 1:0.8:1, or 1:1:1.
[0079] The mass percentage content of a single impurity in the Al-Si aluminum alloy is less than 0.02%, and the sum of the mass percentage content of the impurities is less than 0.1%. Mn, Ti, Cr, and V can be used as impurities, and the sum of their mass percentage content is not more than 0.03%, preferably not more than 0.025%, and more preferably not more than 0.02%.
[0080] The mass percentage content of Mn may be 0-0.01%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, or 0.01%.
[0081] The mass percentage content of Ti may be 0-0.008%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, or 0.008%.
[0082] The mass percentage content of Cr may be 0-0.008%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, or 0.008%.
[0083] The mass percentage content of V may be 0-0.008%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, or 0.008%.
[0084] In one embodiment, the Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.05% Zn by mass, 0.01-0.09% Ni by mass, 0.0009-0.01% B by mass, 0.001-0.01% Mn by mass, 0.001-0.008% Ti by mass, 0.001-0.008% Cr by mass, and 0.001-0.008% V by mass.
[0085] In another embodiment, the Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.04% Zn by mass, 0.01-0.09% Ni by mass, 0.0009-0.01% B by mass, 0.001-0.005% Mn by mass, 0.002-0.005% Ti by mass, 0.002-0.005% Cr by mass, and 0.002-0.005% V by mass.
[0086] In the technical solution of the present invention, the Al-Si aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass. Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, and on the basis of ensuring that the Al-Si aluminum alloy has better formability, it also has excellent mechanical properties and thermal conductivity. The details are as follows:
[0087] (1) When the mass percentage of Si is 5-8%, on the one hand, Si can improve the fluidity and density of aluminum alloy, thereby improving the forming performance and mechanical properties of aluminum alloy. On the other hand, Si can react with other elements to form a second phase as much as possible to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of aluminum alloy. Specifically, Si can react with Al, Fe, Cu, Mg, Mn, B, etc. to form Mg 2 Second phases such as Si, AlFeSi, AlMnSi, AlFeSiCu, AlFeMgSi, AlFeSiB, AlFeMnSi;
[0088] (2) When the mass percentage of Fe is 0.4-0.8%, on the one hand, Fe can reduce the sticking tendency of aluminum alloy castings and improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Fe can react with other elements to form a second phase as much as possible to avoid the adverse effect of Fe dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Fe can react with Al, Si, Mg, Cu, Mn, Ni, B, etc. to form Al 3 Fe, AlFeSi, AlFeMgSi, AlFeSiB, AlFeSiCu, AlFeSiNi, AlFeMgSiNi, AlFeMnSi, FeNiAl 9 Wait for the second phase;
[0089] (3) When the mass percentage of Cu is 0.001-0.05%, on the one hand, Cu can improve the mechanical properties, thermal conductivity, and fatigue resistance of aluminum alloys, and on the other hand, Cu can react with other elements as much as possible to form a second phase to avoid the adverse effect of Cu dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Cu can react with Al, Fe, Si, Mg, Zn, etc. to form CuAl 2 、AlFeSiCu、Al 2 CuZn, (CuMg)Al 2 In addition, Cu can also promote Mg 2 Si、Mg 2 Zn、Mg 2 SiZn、(CuMg)Al 2 , AlFeMgSi, AlFeMgSiNi and other second phases are precipitated to increase their volume fraction and dispersion degree, so as to reduce the solid solubility of the above elements in the aluminum matrix;
[0090] (4) When the mass percentage of Mg is 0.001-0.05%, on the one hand, Mg can improve the mechanical properties and thermal conductivity of aluminum alloys, and on the other hand, Mg can react with other elements to form a second phase as much as possible to avoid the adverse effect of Mg dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Mg can react with Al, Fe, Si, Cu, Zn, Ni, etc. to form Mg 2 Si、Mg 2 Zn、Mg 2 SiZn、(CuMg)Al 2 , AlFeMgSi, AlFeMgSiNi and other second phases. In addition, Mg can also promote CuAl 2 、AlFeSiCu、Al 2 CuZn, (CuMg)Al 2 The precipitation of the second phase, etc., increases its volume fraction and dispersion, thereby reducing the solid solubility of the above elements in the aluminum matrix;
[0091] (5) When the mass percentage of Sr is 0.005-0.04%, on the one hand, Sr can be modified through the heterogeneous nucleation theory or twin valley mechanism to refine the second phase such as eutectic silicon, improve the thermal conductivity and mechanical properties of the aluminum alloy, and transform the β-AlFeSi phase in the ingot into the Chinese character α-AlFeSi phase to improve the mechanical properties of the aluminum alloy. On the other hand, Sr can preferentially combine with Fe, Cu, Mn, Cr, Si and other elements to form dispersion strengthening to avoid the adverse effect of Sr dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. In addition, Sr can also promote CuAl 2 Mg 2 The precipitation of Si and other phases reduces the solid solubility of these alloy elements in the aluminum matrix;
[0092] (6) When the mass percentage of Zn is 0.001-0.1%, on the one hand, Zn can improve the mechanical properties of aluminum alloys, and on the other hand, Zn can react with other elements to form a second phase as much as possible to avoid the adverse effect of Zn dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Zn can react with Al, Mg, Cu and Si to form MgZn 2 Mg 2 SiZn、Al 2 CuZn and other secondary phases. In addition, Zn can eliminate Si to reduce the adverse effects of Si on the performance of aluminum alloys. Zn can also promote Mg 2 Si、Al 2 The precipitation of Cu and other phases improves mechanical properties and thermal conductivity;
[0093] (7) When the mass percentage of Ni is 0.01-0.2%, Ni can be used to improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Ni can be made to react with other elements to form a second phase as much as possible to avoid the adverse effect of Ni dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Ni can react with Al, Fe, Mg, Si, etc. to form Al 3 Ni, AlFeSiNi, AlFeMgSiNi, FeNiAl 9 The second phase promotes the precipitation of elements such as Cu, Mg, Zn, Si, and Fe dissolved in the alloy; Ni can also refine the grains and promote the CuAl 2 、(CuMg)Al 2 Mg 2 The precipitation of strengthening phases such as Si increases the volume fraction and dispersion of the precipitated phase to reduce the solid solubility of alloy elements in the aluminum matrix. In addition, Ni, Cu and Mg can promote each other's precipitation to improve the thermal conductivity and mechanical properties of aluminum alloys.
[0094] (8) When the mass percentage content of B is 0.0008-0.01%, on the one hand, B can react with transition elements Ti, Mn, Cr, V, etc. that sharply reduce the thermal conductivity to form borides. The borides are removed during slagging and sedimentation after the melt is left to stand, thereby reducing the content of Ti, Mn, Cr, and V in the melt. On the other hand, B can also react with other elements to form a second phase as much as possible to avoid the adverse effect of B dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, B can react with Al, Fe, Si, Mn, etc. g, Cu and other reactions generate AlFeSiB, MgB, CuB and other secondary phases, which can not only reduce the solubility of the above elements in the matrix, but also increase the proportion of the precipitated phases of these elements, thereby improving the mechanical properties of the aluminum alloy and the thermal conductivity of the aluminum alloy. In addition, B can also refine the grains, modify and refine the elemental Si to reduce the adverse effects of coarse elemental Si on the performance of the aluminum alloy, and can also transform the β-AlFeSi phase into the Chinese character α-AlFeSi phase to eliminate the adverse effects of the iron-rich phase on the performance of the aluminum alloy, and can inhibit the Ti 3 Segregation of Al.
[0095] Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, which can remove the content of transition elements Ti, Mn, Cr, and V in the aluminum matrix that have a great impact on thermal conductivity, refine the grains, reduce the solid solubility of alloy elements in the aluminum matrix, and increase the volume fraction of the precipitated phase, so as to reduce the adverse effects of alloy elements on the thermal conductivity of aluminum alloys and improve the comprehensive properties of aluminum alloys (including mechanical properties, thermal conductivity, and forming properties, etc.). At the same time, under the further action of aging treatment, the solid solubility of each element in the aluminum matrix is further reduced, which can eliminate the adverse effects of alloy elements on the thermal conductivity of aluminum alloys as much as possible, and the second phase (such as Al 3 Fe、Mg 2 Si、Al 2 Cu, AlFeSiNi, AlMnSi, etc.) can also be refined in the aluminum matrix and at the grain boundaries or within the grain boundaries, greatly improving the mechanical properties and thermal conductivity of the aluminum alloy.
[0096] Specifically, since transition elements such as Mn, Cr, Ti, and V have a great influence on the thermal conductivity and mechanical properties of aluminum alloys, their content needs to be strictly controlled; when the amount of elements such as Cu, Mg, Zn, and B added is large, the thermal conductivity and mechanical properties of the aluminum alloy will also be reduced, and their content also needs to be controlled; but when the mass percentage content of at least one of Cu, Mg, Zn, B, Mn, Cr, Ti, and V is low, the elements with a low mass percentage content are not easy to precipitate, and will exist in the aluminum matrix in the form of solid solution, thereby reducing the thermal conductivity and mechanical properties of the aluminum alloy, and the refinement and modification effect of the aluminum alloy will also deteriorate, causing the single Si at the grain boundary of the aluminum alloy to exist in the form of coarse flakes and strips, seriously splitting the aluminum matrix, and further reducing the thermal conductivity and mechanical properties of the aluminum alloy. In the technical solution of the present invention, as described in the above items (1) to (8), Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, which can refine the grains (such as the modification effect of Sr, the grain refining effect of Ni and B), reduce each other's solid solubility in the aluminum matrix (such as the elements can react with each other to form a second phase), and increase the volume fraction of the precipitated phase (such as Cu, Mg, Sr, Zn, and Ni can promote the precipitation of the second phase), so as to improve the mechanical properties and thermal conductivity of the aluminum alloy; even if the mass percentage content of one or some elements is low, during the aging treatment process, all or almost all of the elements can be precipitated, avoiding adverse effects on the thermal conductivity of the aluminum alloy.
[0097] It is understandable that, since the addition of alloying elements will reduce the thermal conductivity of aluminum alloys, the addition amount of at least one element among Si, Fe, Cu, Mg, Sr, Zn, Ni, and B in the present invention may be less than the addition amount of the element in the prior art, wherein the addition amount of all elements among Si, Fe, Cu, Mg, Sr, Zn, Ni, and B in the present invention may be less than the addition amount of the elements in the prior art. Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact and influence each other as a whole, which can avoid the addition of too many elements to reduce the thermal conductivity of aluminum alloys on the one hand, and on the other hand, at least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, and B can still improve the comprehensive properties of aluminum alloys (including mechanical properties and thermal conductivity, etc.) when the addition amount is small.
[0098] The Al-Si aluminum alloy also contains 0-0.009% In by mass, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, or 0.009%.
[0099] The mass ratio of Cu to In is 0.1-20:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties of the aluminum alloy gradually increase. The mass ratio of Cu to In is preferably 1-20:1, more preferably 5-10:1, specifically 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, or 20:1.
[0100] In the technical solution of the present invention, the Al-Si aluminum alloy further contains 0-0.009% by mass of In. On the one hand, In can improve the mechanical properties of the aluminum alloy. On the other hand, In can react with other elements as much as possible to form a second phase to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, In can react with Al and Cu to form second phases such as AlIn and CuIn. In can also refine the grains to improve the elongation of the aluminum alloy.
[0101] The Al-Si aluminum alloy further contains Nb in an amount of 0-0.005% by mass, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005% by mass.
[0102] The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, B, Nb, and RE is 5.6-9%, preferably 6-8.9%, more preferably 6.5-8%, and specifically may be 5.6%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, or 9%.
[0103] The mass ratio of Ni to Nb is 1-50:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Ni to Nb is preferably 10-40:1, more preferably 20-30:1, and specifically can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 12:1, 14:1, 16:1, 18:1, 20:1, 22:1, 24:1, 26:1, 28:1, 30:1, 32:1, 34:1, 36:1, 38:1, 40:1, 42:1, 44:1, 46:1, 48:1, or 50:1. The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, Nb and Sb is 5.5-9%, preferably 6-8%, more preferably 6-7%, and specifically may be 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, or 9%.
[0104] In the technical solution of the present invention, the Al-Si aluminum alloy further contains 0-0.005% by mass of Nb. On the one hand, Nb can improve the mechanical properties and thermal conductivity of the aluminum alloy. On the other hand, Nb can react with other elements as much as possible to form a second phase to avoid the adverse effect of Nb dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Nb can react with Ti and Al to form a TiAl-Nb phase. In addition, Nb can also refine the grains to improve the elongation of the aluminum alloy.
[0105] The Al-Si aluminum alloy further contains Bi in an amount of 0-0.006% by mass, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, or 0.006% by mass.
[0106] The mass ratio of Mg to Bi is 10-450:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties of the aluminum alloy gradually increase. The mass ratio of Mg to Bi is preferably 50-400:1, more preferably 100-300:1, and more preferably 150-200:1, and specifically can be 10:1, 50:1, 100:1, 150:1, 200:1, 250:1, 300:1, 350:1, 400:1, or 450:1.
[0107] In the technical solution of the present invention, the Al-Si aluminum alloy further contains Bi in a mass percentage content of 0-0.006%. On the one hand, Bi can improve the mechanical properties of the aluminum alloy, and on the other hand, Bi can react with other elements as much as possible to form a second phase to avoid the adverse effect of Bi dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Bi can react with Mg and Cd to form Mg 3 Bi 2 Mg 3 (BiCd) 2 Wait for the second phase.
[0108] The Al-Si aluminum alloy further contains Ge in an amount of 0-0.005% by mass, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005% by mass.
[0109] The mass ratio of Si to Ge is 1000-2000:1. Within the range of this mass ratio, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Ge is preferably 1000-1500:1, more preferably 1300-1500:1, and specifically can be 1000:1, 1100:1, 1200:1, 1300:1, 1400:1, 1500:1, 1600:1, 1700:1, 1800:1, 1900:1, 2000:1.
[0110] In the technical solution of the present invention, the Al-Si aluminum alloy further contains Ge in a mass percentage content of 0-0.005%. On the one hand, Ge can improve the mechanical properties and thermal conductivity of the aluminum alloy. On the other hand, Ge can react with other elements as much as possible to form a second phase to avoid the adverse effect of Ge dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Ge can react with Al and Si to form Al 9 Ge 7 、Al 6 Ge 5 、Al 5 Ge 2 、Al 3 Ge 4 , SiGe and other second phases. In addition, Ge can promote Mg 2 Si、CuAl 2 The precipitation of the second phase, such as Ge, can refine the precipitated phase to reduce the solid solubility of the above elements in the aluminum matrix. Ge can also replace part of Si atoms in the metastable precipitated phase. The Si-Ge phase precipitated at the beginning of aging provides a nucleation site for the θ phase, increasing the density of the θ phase, thereby further improving the mechanical properties and thermal conductivity of the aluminum alloy.
[0111] The Al-Si aluminum alloy further contains 0-0.005% by mass of Mo, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%.
[0112] The mass ratio of Si to Mo is 1500-2000:1. Within the mass ratio range, as the mass ratio decreases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Si to Mo is preferably 1500-1800:1, more preferably 1500-1600:1, specifically 1500:1, 1600:1, 1700:1, 1800:1, 1900:1, or 2000:1.
[0113] In the technical solution of the present invention, the Al-Si aluminum alloy also contains 0-0.005% Mo by mass. On the one hand, Mo can improve the mechanical properties and thermal conductivity of the aluminum alloy. On the other hand, Mo can react with other elements to form a second phase as much as possible to avoid the adverse effect of Ge dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Mo can react with Al, Si, Fe, etc. to form AlMo, AlSiMo, AlSiFeMo and other second phases, which are dispersed in the aluminum matrix grain boundaries. In addition, Mo can also refine the grains, improve the morphology of Fe-containing intermetallic compounds, and further improve the mechanical properties of the aluminum alloy.
[0114] The Al-Si aluminum alloy further contains Ag in an amount of 0-0.005% by mass, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.003%, 0.004%, or 0.005% by mass.
[0115] The mass ratio of Mg to Ag is 10-500:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg to Ag is preferably 50-400:1, more preferably 100-300:1, and more preferably 200-300:1. Specifically, it can be 10:1, 50:1, 100:1, 150:1, 200:1, 250:1, 300:1, 350:1, 400:1, 450:1, or 500:1.
[0116] The mass ratio of Cu to Ag is 10-400:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Cu to Ag is preferably 50-300:1, more preferably 100-200:1, specifically 10:1, 50:1, 100:1, 150:1, 200:1, 250:1, 300:1, 350:1, or 400:1.
[0117] In the technical solution of the present invention, the Al-Si aluminum alloy also contains 0-0.005% Ag by mass, which can promote the second phase (such as Al 2 Cu、Mg 2 Si、Mg 2 Sb、Mg 3 Sn 2 , and Mg 3 Bi 2 The precipitation of aluminum alloy can be improved by refining the precipitation phase and increasing the density of the precipitation phase, thereby improving the precipitation strengthening effect of the aluminum alloy and thus improving the mechanical properties and thermal conductivity of the aluminum alloy.
[0118] The Al-Si aluminum alloy further contains Sn in an amount of 0-0.1% by mass and Te in an amount of 0-0.005% by mass.
[0119] The mass ratio of Mg to Sn is 0.3-10:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Mg to Sn is preferably 0.5-8:1, more preferably 1-8:1, and more preferably 5-8:1, and specifically can be 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, or 10:1.
[0120] The mass ratio of Te to Sn is 0.01-1:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Te to Sn is preferably 0.05-1:1, more preferably 0.1-8:1, and more preferably 1-5:1, and specifically can be 0.01:1, 0.02:1, 0.04:1, 0.06:1, 0.08:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, or 1:1.
[0121] In the technical solution of the present invention, the Al-Si aluminum alloy also contains 0-0.1% Sn by mass and 0-0.005% Te by mass. Te can improve the mechanical properties and thermal conductivity of aluminum alloys. Te can narrow the solidification temperature range of aluminum alloys, form tiny petal-shaped rather than dendritic primary crystals, reduce or eliminate micro-shrinkage, and thus improve the mechanical properties and thermal conductivity of aluminum alloys. Sn can improve the thermal conductivity of aluminum alloys, and can also react with other elements as much as possible to generate a second phase to avoid the adverse effects of Ge dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Sn can react with Al to generate Al 9 Sn 7 、Al 6 Sn 5 、Al 5 Sn 2 、Al 3 Sn 4 And other high temperature strengthening phases.
[0122] The Al-Si aluminum alloy further contains 0-0.01% Be by mass and 0-0.1% Co by mass. The Be by mass content may be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, or 0.01%. The Co by mass content may be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, or 0.1%.
[0123] The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, B, Mo, In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE is 5.7-9.2%, preferably 6-9%, and more preferably 6.5-7%, and specifically may be 5.7%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.1% or 9.2%.
[0124] The mass ratio of Be, Co, and Fe is 0.001-0.03:0.004-0.25:1. Within this mass ratio range, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of Be, Co, and Fe is preferably 0.005-0.02:0.005-0.2:1, more preferably 0.01-0.015:0.01-0.05:1, specifically 0.001:0.004:1, 0.001:0.01:1, 0.001:0.05:1, 0.001:0.1:1, 0.001:0.2:1, 0.001:0.25:1, 0.005:0.004:1, 0.005:0.01:1, 0.005:0.05:1, 0.005:0.1:1, 0.005:0.2:1, 0.005:0 .25:1, 0.01:0.004:1, 0.01:0.01:1, 0.01:0.05:1, 0.01:0.1:1, 0.01:0.2:1, 0.01:0.25:1, 0.02:0.004:1, 0.02:0.01:1, 0.02:0.05:1, 0.02:0.1:1, 0.02:0.2:1, 0.02:0.25:1, 0.03:0.004:1, 0.03:0.01:1, 0.03:0.05:1, 0.03:0.1:1, 0.03:0.2:1, or 0.03:0.25:1.
[0125] The mass ratio of Fe to Co is 1-250:1. Within this mass ratio range, as the mass ratio increases, the thermal conductivity of the aluminum alloy gradually increases. The mass ratio of Fe to Co is preferably 10-80:1, more preferably 30-50:1, and specifically can be 1:1, 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1, 80:1, 85:1, 90:1, 95:1, 100:1, 110:1, 120:1, 130:1, 140:1, 150:1, 160:1, 170:1, 180:1, 190:1, 200:1, 210:1, 220:1, 230:1, 240:1, or 250:1.
[0126] In the technical solution of the present invention, the Al-Si aluminum alloy further contains 0-0.01% Be by mass and 0-0.1% Co by mass. Be can transform the eutectic Si phase from a lamellar phase to a fine phase to refine the Si phase, thereby reducing or eliminating the adverse effects of Si on the aluminum alloy, and can transform the plate-like β intermediate phase into a relatively harmless Chinese character-shaped Be-Fe (Al 8 Fe2 SiBe) phase can reduce or eliminate the adverse effects of Fe on the performance of aluminum alloys. Secondly, it can reduce the formation of Mg-rich Fe phase, thereby increasing the Mg content in the aging process. Be can also combine with vacancies to prevent vacancies from migrating and disappearing. The addition of Be significantly increases the nucleation rate of metastable phases, improves the strengthening effect of aging, and reduces the solubility of the above elements in the aluminum matrix. Ni and Be are combined to greatly promote the precipitation of the second phase and reduce the solubility of alloy elements in the matrix. On the one hand, Co can refine the grains to improve the thermal conductivity and mechanical properties of aluminum alloys. On the other hand, it can react with other elements as much as possible to generate the second phase to avoid the adverse effects of Be dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Co can react with Al, Fe, Si, etc. to generate Al 15 (Fe,Co) 3 Si 2 、Al 3 (Fe, Co) and other second phases. In addition, Co to Al 3 The Fe phase has a refining effect, which can refine the coarse needle-shaped and flake-shaped β-Al 3 Fe phase transforms into small flower-like and fine strip-shaped α-Al 15 (Fe,Co) 3 Si 2 phase, and can also promote the α-Al 15 (Fe,Co) 3 Si 2 The precipitation of phase further improves the mechanical properties and thermal conductivity of aluminum alloy. The composite addition of Ni and Co can effectively modify Fe and transform free Fe into the second phase. The composite addition of Co, Ni and Be can quickly reduce the solid solubility of each other in the alloy and increase the volume fraction of the second phase to improve the mechanical properties and thermal conductivity of aluminum alloy.
[0127] The Al-Si aluminum alloy further contains 0-0.01% by mass of Cd and 0-0.02% by mass of RE, wherein RE is at least one of La, Ce, Pr, Nd, Er, Sm, Y, and Gd.
[0128] The mass percentage content of Cd may be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, or 0.01%.
[0129] The mass percentage content of RE may be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, or 0.02%.
[0130] The mass ratio of RE, Sr, and Fe is 0.002-0.1:0.02-0.08:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of RE, Sr, and Fe is preferably 0.005-0.05:0.04-0.06:1, and more preferably 0.01-0.03:0.05-0.06:1, and specifically 0.002:0.02:1, 0.002:0.04:1, 0.002:0.06:1, 0.002:0.08:1, 0.005:0.02:1, 0.005:0.04:1, 0.005:0.0 6:1, 0.005:0.08:1, 0.01:0.02:1, 0.01:0.04:1, 0.01:0.06:1, 0.01:0.08:1, 0.05:0.02:1, 0.05:0.04:1, 0.05:0.06:1, 0.05:0.08:1, 0.1:0.02:1, 0.1:0.04:1, 0.1:0.06:1, or 0.1:0.08:1.
[0131] The mass ratio of RE, B, and Fe is 0.002-0.1:0.0001-0.03:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of RE, B, and Fe is preferably 0.005-0.08:0.0005-0.02:1, and more preferably 0.01-0.03:0.01-0.02:1, and specifically 0.002:0.0001:1, 0.002:0.0005:1, 0.002:0.01:1, 0.002:0.03:1, 0.005:0.0001:1, 0.005:0.0005:1, 0.005:0.01:1, 0.005:0.0005:1, 0.005:0.01:1 : 1, 0.005:0.03:1, 0.01:0.0001:1, 0.01:0.0005:1, 0.01:0.01:1, 0.01:0.03:1, 0.05:0.0001:1, 0.05:0.0005:1, 0.05:0.01:1, 0.05:0.03:1, 0.1:0.0001:1, 0.1:0.0005:1, 0.1:0.01:1, or 0.1:0.03:1.
[0132] The mass ratio of RE to Cd is 0.1-25:1. Within this mass ratio range, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of RE to Cd is preferably 1-20:1, more preferably 5-20:1, and more preferably 10-15:1. Specifically, it can be 0.1:1, 0.5:1, 1:1, 5:1, 10:
[0133] 1, 15:1, 20:1, or 25:1.
[0134] The mass ratio of RE, B, and Be is 0.5-20:0.1-10:1. Within the range of this mass ratio, as the mass ratio increases, the mechanical properties and thermal conductivity of the aluminum alloy gradually increase. The mass ratio of RE, B, and Be is preferably 1-20:0.5-10:1, more preferably 5-10:1-5:1, specifically 0.5:0.1:1, 0.5:0.5:1, 0.5:1:1, 0.5:5:1, 0.5:10:1, 1:0.1:1, 1:0.5:1, 1:1:1, 1:5:1, 1:10:1, 5:0.1:1, 5:0.5 :1, 5:1:1, 5:5:1, 5:10:1, 10:0.1:1, 10:0.5:1, 10:1:1, 10:5:1, 10:10:1, 15:0.1:1, 15:0.5:1, 15:1:1, 15:5:1, 15:10:1, 20:0.1:1, 20:0.5:1, 20:1:1, 20:5:1, or 20:10:1.
[0135] In the technical solution of the present invention, the Al-Si aluminum alloy also contains 0-0.01% Cd by mass and 0-0.02% RE by mass. RE can refine the alloy structure to improve the mechanical properties of the aluminum alloy, and can also form a rare earth active film on the surface of the Fe-containing phase or combine with Al, Fe, Ti and other atoms to form rare earth compounds to effectively reduce the solid solution of harmful elements in the aluminum matrix. RE can also transform the long strip β-Fe phase into a spherical α-Fe phase and modify the elemental Si. RE can also promote the dispersion phase such as CuAl 2 、(CuMg)Al 2 RE can also refine the grains, second phases and precipitation phases (e.g., it can refine Al 3 R E, A L 3 Fe、Mg 2 Si phase), further improving the mechanical properties and thermal conductivity of aluminum alloys. Cd can refine α-Al and form REAl with Al, RE, Cu, Mg, Si, Fe, and Bi. 2 Cd 3 、Al 3 Cd、Al 2 Cd 3 、(CuCd)Al 2 Mg 2 (SiCdREFe), Mg 3 (BiCd) 2 In addition, Cd will form a large number of Cd-vacancy clusters during the aging stage, which will promote and accelerate the CuAl 2 The solid solubility of the above elements in the aluminum matrix can be reduced by the precipitation of the phase.
[0136] In one embodiment, the Al-Si aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, 0.0008-0.01% B by mass, 0.0001-0.009% In by mass, 0.0001-0.005% Nb by mass, The content of Bi is 0.0001-0.006% by mass, the content of Ge is 0.0001-0.005% by mass, the content of Mo is 0.0001-0.005% by mass, the content of Ag is 0.0001-0.005% by mass, the content of Sn is 0.0001-0.1% by mass, the content of Te is 0.0001-0.005% by mass, the content of Be is 0.0001-0.01% by mass, the content of Co is 0.001-0.1% by mass, the content of Cd is 0.001-0.01% by mass, and the content of RE is 0.001-0.02% by mass.
[0137] In one embodiment, the Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.04% Zn by mass, 0.01-0.09% Ni by mass, 0.0009-0.01% B by mass, 0.001-0.01% Mn by mass, 0.001-0.008% Ti by mass, 0.001-0.008% Cr by mass, 0.001-0.008% V by mass, and 0.001-0.008% Ti by mass. The content of In is 0.0001-0.009% by mass, the content of Nb is 0.0001-0.005% by mass, the content of Bi is 0.0001-0.006% by mass, the content of Ge is 0.0001-0.005% by mass, the content of Mo is 0.0001-0.005% by mass, the content of Ag is 0.0001-0.005% by mass, the content of Sn is 0.0001-0.1% by mass, the content of Te is 0.0001-0.005% by mass, the content of Be is 0.0001-0.01% by mass, the content of Co is 0.001-0.1% by mass, the content of Cd is 0.001-0.01% by mass, and the content of RE is 0.001-0.02% by mass.
[0138] In another embodiment, the Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.04% Zn by mass, 0.01-0.09% Ni by mass, 0.0009-0.01% B by mass, 0.001-0.005% Mn by mass, 0.002-0.005% Ti by mass, 0.002-0.005% Cr by mass, 0.002-0.005% V by mass, and 0.006-0.01% Ti by mass. The content of In is 0.0001-0.005% by mass, the content of Nb is 0.0001-0.003% by mass, the content of Bi is 0.0001-0.005% by mass, the content of Ge is 0.0001-0.004% by mass, the content of Mo is 0.0001-0.002% by mass, the content of Ag is 0.0001-0.002% by mass, the content of Sn is 0.0001-0.05% by mass, the content of Te is 0.0001-0.003% by mass, the content of Be is 0.0001-0.005% by mass, the content of Co is 0.001-0.05% by mass, the content of Cd is 0.001-0.005% by mass, and the content of RE is 0.001-0.01% by mass.
[0139] The present invention also provides a method for preparing an Al-Si series aluminum alloy, comprising the following steps:
[0140] The aluminum source is heated at a temperature of 720-780° C. to obtain aluminum liquid, wherein the aluminum liquid contains Mn, Cr, Ti, and V;
[0141] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and B to the aluminum liquid, performing a second heating treatment, and keeping the temperature at 700-750° C. for 10-30 minutes to obtain an alloy liquid;
[0142] After refining, degassing, and slagging the alloy liquid, the composition and content are tested; and
[0143] After the composition and content are tested to be qualified, the alloy liquid is subjected to die casting and aging treatment to obtain an Al-Si aluminum alloy. The Al-Si aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass.
[0144] The aluminum source is at least one of original aluminum, aluminum ingot, and recycled aluminum.
[0145] The liquid aluminum produced by industrial aluminum electrolytic cells is purified, clarified and deslagging, and then cast into commercial aluminum ingots. The aluminum content generally does not exceed 99.8%, which is called primary aluminum.
[0146] Aluminum ingots are made of pure aluminum and recycled aluminum as raw materials. Other elements such as Si, Cu, Mg, Fe, etc. are added according to international standards or special requirements to improve the deficiencies of pure aluminum in castability, chemical properties and physical properties.
[0147] Recycled aluminum, also known as "secondary aluminum", is an aluminum alloy or aluminum metal obtained by remelting and refining scrap aluminum, scrap aluminum alloy materials, or aluminum-containing scrap. The main raw materials for smelting recycled aluminum are industrial scrap aluminum parts (such as aircraft scrap parts and engines, casing covers, etc.) and scrap aluminum materials generated during aluminum processing (including plates, pipes, bars, profiles, scraps, foils, etc.).
[0148] It can be understood that the aluminum source may also be an aluminum source other than original aluminum, aluminum ingot, and recycled aluminum.
[0149] Impurities commonly contained in the aluminum source include Mn, Ti, Cr, or V.
[0150] At least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, and B may be added in the form of an alloy or a single substance.
[0151] The preparation method of the Al-Si aluminum alloy further includes the step of adding at least one of In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE to the aluminum liquid. At least one of In, Nb, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, Cd, and RE can be added in the form of an alloy or a single substance. The mass percentage content of In can be 0-0.009%. The mass percentage content of Nb is 0-0.005%. The mass percentage content of Bi can be 0-0.006%. The mass percentage content of Ge can be 0-0.005%. The mass percentage content of Mo can be 0-0.005%. The mass percentage content of Ag can be 0-0.005%. The mass percentage content of Sn can be 0-0.1%. The mass percentage content of Te can be 0-0.005%. The mass percentage content of Be can be 0-0.01%. The mass percentage content of Co can be 0-0.1%. The mass percentage content of Cd can be 0-0.01%. The mass percentage content of RE can be 0-0.02%, and RE is at least one of La, Ce, Pr, Nd, Er, Sm, Y, and Gd.
[0152] In one embodiment, the aging treatment temperature is 280 to 350°C, and the time is 0.05h to 15h. The aging treatment temperature can be 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, or 350°C; the aging treatment time can be 0.05h, 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.5h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, or 15h. During the aging treatment, the size of the precipitated phase gradually changes to a smaller size, and all or almost all of the alloying elements dissolved in the alloy are precipitated, increasing the pinning effect on dislocations and greatly improving the thermal conductivity and mechanical properties of the aluminum alloy.
[0153] In another embodiment, the aging treatment, which may also be referred to as a multi-stage aging treatment, includes a primary low-temperature aging treatment, a secondary low-temperature aging treatment, and a tertiary high-temperature aging treatment. The temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1 to 15 hours; the temperature of the secondary low-temperature aging treatment is 0 to 70°C, and the time is 1 to 24 hours; the temperature of the tertiary high-temperature aging treatment is 280 to 350°C, and the time is 0.05 to 15 hours. The temperature of the primary low-temperature aging treatment may specifically be -200°C, -190°C, -180°C, -170°C, -160°C, -150°C, -140°C, -130°C, -120°C, -110°C, or -100°C. The time of the primary low-temperature aging treatment may be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, or 15h. The temperature of the secondary low-temperature aging treatment may be 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, or 70°C. The time of the secondary low-temperature aging treatment may be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, or 24h. The temperature of the three-stage high-temperature aging treatment may specifically be 280° C., 285° C., 290° C., 295° C., 300° C., 305° C., 310° C., 315° C., 320° C., 325° C., 330° C., 335° C., 340° C., 345° C., or 350° C. The time of the three-stage high-temperature aging treatment may specifically be 0.05h, 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.5h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, or 15h.
[0154] During the first-level low-temperature aging treatment, deep cryogenic treatment can inhibit the segregation of atoms such as Mg, Cu, Ni and Si, and at the same time make the alloy produce a greater degree of supercooling, significantly increase the range of the GP zone, facilitate the subsequent high-temperature process nucleation rate to increase, and the alloy elements can be more fully precipitated. Aluminum alloys also undergo volume and lattice contraction during low-temperature processes, the supersaturation of alloy elements increases, solute atoms will precipitate in the alloy, and the content of alloy elements participating in aging will be increased. In addition, the reduction in the solubility of solute atoms will cause solute atoms to segregate at dislocations, significantly improving the formation of GP zones. During the second-level low-temperature aging treatment, the atomic segregation under the action of internal stress and dislocation will be uniformly diffused and dispersed in the aluminum matrix and grain boundaries. During the three-level high-temperature aging treatment, the GP zone gradually transforms into a precipitation phase with a smaller size but a larger volume fraction, and all or nearly all of the alloy elements dissolved in the alloy are precipitated, increasing the pinning effect on dislocations, greatly improving the thermal conductivity and mechanical properties of aluminum alloys.
[0155] The alloy liquid is subjected to die casting at a temperature of 660-700°C, wherein the die casting speed of the die casting machine is 0.23-2.5 m / s. It can be understood that the die casting process of the present invention is a common die casting process, and vacuum die casting can also be used to die cast the alloy liquid. The strength (such as yield strength and tensile strength) and elongation of the aluminum alloy after vacuum die casting will be higher than the strength (such as yield strength and tensile strength) and elongation of the aluminum alloy after common die casting.
[0156] The temperature of the refining treatment is 690-750°C and the time is 10-20 minutes. The refining agent of the refining treatment may include the following raw materials in parts by weight: 60-70 parts of KF, 50-60 parts of NaCl, 40-60 parts of LiCl, 20-25 parts of cryolite, 10-25 parts of AIF3, 10-15 parts of CaF2, 5-10 parts of light calcium carbonate, 15-20 parts of graphite powder, 10-20 parts of talc, 20-30 parts of MgCl2, and 10-30 parts of rare earth acid salt. The rare earth acid salt may be one of the chlorides, fluorides, and nitric acid compounds of light rare earths, or a combination thereof. The rare earth acid salt may be one of the chlorides, fluorides, and nitric acid compounds of heavy rare earths, or a combination thereof. The mass ratio of the refining agent to the alloy liquid is 0.0013-0.0018:1.
[0157] It is understandable that when the content of each component in the alloy liquid after degassing and slag removal treatment meets the standard, subsequent treatments such as die casting are performed. Among them, the aluminum alloy that meets the standard contains Si with a mass percentage content of 5-8%, Fe with a mass percentage content of 0.4-0.8%, Cu with a mass percentage content of 0.001-0.05%, Mg with a mass percentage content of 0.001-0.05%, Sr with a mass percentage content of 0.005-0.04%, Zn with a mass percentage content of 0.001-0.1%, Ni with a mass percentage content of 0.01-0.2%, B with a mass percentage content of 0.0008-0.01%, and Al and unavoidable impurities. When the composition and content are unqualified, the corresponding elements can be added to adjust until the composition and content are qualified.
[0158] In the technical solution of the present invention, the Al-Si aluminum alloy prepared by the preparation method of the Al-Si aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.2% Ni by mass, and 0.0008-0.01% B by mass. Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, and have excellent mechanical properties and thermal conductivity on the basis of ensuring that the Al-Si aluminum alloy has better formability. The details are as follows:
[0159] (1) When the mass percentage of Si is 5-8%, on the one hand, Si can improve the fluidity and density of aluminum alloy, thereby improving the forming performance and mechanical properties of aluminum alloy. On the other hand, Si can react with other elements to form a second phase as much as possible to avoid the adverse effect of Si dissolved in the aluminum matrix on the thermal conductivity of aluminum alloy. Specifically, Si can react with Al, Fe, Cu, Mg, Mn, B, etc. to form Mg 2 Second phases such as Si, AlFeSi, AlMnSi, AlFeSiCu, AlFeMgSi, AlFeSiB, AlFeMnSi;
[0160] (2) When the mass percentage of Fe is 0.4-0.8%, on the one hand, Fe can reduce the sticking tendency of aluminum alloy castings and improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Fe can react with other elements to form a second phase as much as possible to avoid the adverse effect of Fe dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Fe can react with Al, Si, Mg, Cu, Mn, Ni, B, etc. to form Al 3 Fe, AlFeSi, AlFeMgSi, AlFeSiB, AlFeSiCu, AlFeSiNi, AlFeMgSiNi, AlFeMnSi, FeNiAl 9 Wait for the second phase;
[0161] (3) When the mass percentage of Cu is 0.001-0.05%, on the one hand, Cu can improve the mechanical properties, thermal conductivity, and fatigue resistance of aluminum alloys, and on the other hand, Cu can react with other elements as much as possible to form a second phase to avoid the adverse effect of Cu dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Cu can react with Al, Fe, Si, Mg, Zn, etc. to form CuAl 2 、AlFeSiCu、Al 2 CuZn, (CuMg)Al 2 In addition, Cu can also promote Mg 2 Si、Mg 2 Zn、Mg 2 SiZn、(CuMg)Al 2 , AlFeMgSi, AlFeMgSiNi and other second phases are precipitated to increase their volume fraction and dispersion degree, so as to reduce the solid solubility of the above elements in the aluminum matrix;
[0162] (4) When the mass percentage of Mg is 0.001-0.05%, on the one hand, Mg can improve the mechanical properties and thermal conductivity of aluminum alloys, and on the other hand, Mg can react with other elements to form a second phase as much as possible to avoid the adverse effect of Mg dissolved in the aluminum matrix on the thermal conductivity of aluminum alloys. Specifically, Mg can react with Al, Fe, Si, Cu, Zn, Ni, etc. to form Mg 2 Si、Mg 2 Zn、Mg 2 SiZn、(CuMg)Al 2 , AlFeMgSi, AlFeMgSiNi and other second phases. In addition, Mg can also promote CuAl 2 、AlFeSiCu、Al 2 CuZn, (CuMg)Al 2 The precipitation of the second phase, etc., increases its volume fraction and dispersion, thereby reducing the solid solubility of the above elements in the aluminum matrix;
[0163] (5) When the mass percentage of Sr is 0.005-0.04%, on the one hand, Sr can be modified through the heterogeneous nucleation theory or twin valley mechanism to refine the second phase such as eutectic silicon, improve the thermal conductivity and mechanical properties of the aluminum alloy, and transform the β-AlFeSi phase in the ingot into the Chinese character α-AlFeSi phase to improve the mechanical properties of the aluminum alloy. On the other hand, Sr can preferentially combine with Fe, Cu, Mn, Cr, Si and other elements to form dispersion strengthening to avoid the adverse effect of Sr dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. In addition, Sr can also promote CuAl 2 Mg 2 The precipitation of Si and other phases reduces the solid solubility of these alloy elements in the aluminum matrix;
[0164] (6) When the mass percentage of Zn is 0.001-0.1%, on the one hand, Zn can improve the mechanical properties of aluminum alloys, and on the other hand, Zn can react with other elements to form a second phase as much as possible to avoid the adverse effect of Zn dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Zn can react with Al, Mg, Cu and Si to form MgZn 2 Mg 2 SiZn、Al 2 CuZn and other secondary phases. In addition, Zn can eliminate Si to reduce the adverse effects of Si on the performance of aluminum alloys. Zn can also promote Mg 2 Si、Al 2 The precipitation of Cu and other phases improves mechanical properties and thermal conductivity;
[0165] (7) When the mass percentage of Ni is 0.01-0.2%, Ni can be used to improve the mechanical properties and thermal conductivity of aluminum alloys. On the other hand, Ni can be made to react with other elements to form a second phase as much as possible to avoid the adverse effect of Ni dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, Ni can react with Al, Fe, Mg, Si, etc. to form Al 3 Ni, AlFeSiNi, AlFeMgSiNi, FeNiAl 9 The second phase promotes the precipitation of elements such as Cu, Mg, Zn, Si, and Fe dissolved in the alloy; Ni can also refine the grains and promote the CuAl 2 、(CuMg)Al 2 Mg 2 The precipitation of strengthening phases such as Si increases the volume fraction and dispersion of the precipitated phase to reduce the solid solubility of alloy elements in the aluminum matrix. In addition, Ni, Cu and Mg can promote each other's precipitation to improve the thermal conductivity and mechanical properties of aluminum alloys.
[0166] (8) When the mass percentage content of B is 0.0008-0.01%, on the one hand, B can react with transition elements Ti, Mn, Cr, V, etc. that sharply reduce the thermal conductivity to form borides. The borides are removed during slagging and sedimentation after the melt is left to stand, thereby reducing the content of Ti, Mn, Cr, and V in the melt. On the other hand, B can also react with other elements to form a second phase as much as possible to avoid the adverse effect of B dissolved in the aluminum matrix on the thermal conductivity of the aluminum alloy. Specifically, B can react with Al, Fe, Si, Mn, etc. g, Cu and other reactions generate AlFeSiB, MgB, CuB and other secondary phases, which can not only reduce the solubility of the above elements in the matrix, but also increase the proportion of the precipitated phases of these elements, thereby improving the mechanical properties of the aluminum alloy and the thermal conductivity of the aluminum alloy. In addition, B can also refine the grains, modify and refine the elemental Si to reduce the adverse effects of coarse elemental Si on the performance of the aluminum alloy, and can also transform the β-AlFeSi phase into the Chinese character α-AlFeSi phase to eliminate the adverse effects of the iron-rich phase on the performance of the aluminum alloy, and can inhibit the Ti 3 Segregation of Al.
[0167] Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, which can remove the content of transition elements Ti, Mn, Cr, and V in the aluminum matrix that have a great impact on thermal conductivity, refine the grains, reduce the solid solubility of alloy elements in the aluminum matrix, and increase the volume fraction of the precipitated phase, so as to reduce the adverse effects of alloy elements on the thermal conductivity of aluminum alloys and improve the comprehensive properties of aluminum alloys (including mechanical properties, thermal conductivity, and forming properties, etc.). At the same time, under the further action of aging treatment, the solid solubility of each element in the aluminum matrix is further reduced, which can eliminate the adverse effects of alloy elements on the thermal conductivity of aluminum alloys as much as possible, and the second phase (such as Al 3 Fe、Mg 2 Si、Al 2 Cu, AlFeSiNi, AlMnSi, etc.) can also be refined in the aluminum matrix and at the grain boundaries or within the grain boundaries, greatly improving the mechanical properties and thermal conductivity of the aluminum alloy.
[0168] Specifically, since transition elements such as Mn, Cr, Ti, and V have a great influence on the thermal conductivity and mechanical properties of aluminum alloys, their content needs to be strictly controlled; when the amount of elements such as Cu, Mg, Zn, and B added is large, the thermal conductivity and mechanical properties of the aluminum alloy will also be reduced, and their content also needs to be controlled; but when the mass percentage content of at least one of Cu, Mg, Zn, B, Mn, Cr, Ti, and V is low, the elements with a low mass percentage content are not easy to precipitate, and will exist in the aluminum matrix in the form of solid solution, thereby reducing the thermal conductivity and mechanical properties of the aluminum alloy, and the refinement and modification effect of the aluminum alloy will also deteriorate, causing the single Si at the grain boundary of the aluminum alloy to exist in the form of coarse flakes and strips, seriously splitting the aluminum matrix, and further reducing the thermal conductivity and mechanical properties of the aluminum alloy. In the technical solution of the present invention, as described in the above items (1) to (8), Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact with each other as a whole, which can refine the grains (such as the modification effect of Sr, the grain refining effect of Ni and B), reduce each other's solid solubility in the aluminum matrix (such as the elements can react with each other to form a second phase), and increase the volume fraction of the precipitated phase (such as Cu, Mg, Sr, Zn, and Ni can promote the precipitation of the second phase), so as to improve the mechanical properties and thermal conductivity of the aluminum alloy; even if the mass percentage content of one or some elements is low, during the aging treatment process, all or almost all of the elements can be precipitated, avoiding adverse effects on the thermal conductivity of the aluminum alloy.
[0169] It is understandable that, since the addition of alloying elements will reduce the thermal conductivity of aluminum alloys, the addition amount of at least one element among Si, Fe, Cu, Mg, Sr, Zn, Ni, and B in the present invention may be less than the addition amount of the element in the prior art, wherein the addition amount of all elements among Si, Fe, Cu, Mg, Sr, Zn, Ni, and B in the present invention may be less than the addition amount of the elements in the prior art. Si, Fe, Cu, Mg, Sr, Zn, Ni, and B within the above content range interact and influence each other as a whole, which can avoid the addition of too many elements to reduce the thermal conductivity of aluminum alloys on the one hand, and on the other hand, at least one of Si, Fe, Cu, Mg, Sr, Zn, Ni, and B can still improve the comprehensive properties of aluminum alloys (including mechanical properties and thermal conductivity, etc.) when the addition amount is small.
[0170] The present invention also provides a heat dissipation structure. At least part of the heat dissipation structure is made of the Al-Si aluminum alloy or the Al-Si aluminum alloy prepared by the preparation method of the Al-Si aluminum alloy. The heat dissipation structure has excellent thermal conductivity and mechanical properties. The Al-Si aluminum alloy has excellent elongation, so that the Al-Si aluminum alloy can be suitable for various processes to make different structural parts.
[0171] The heat dissipation structure can be a filter housing of a communication base station, a heat dissipation substrate of a communication base station, a cabinet shell of a communication base station, a three-electric structural component housing of a car, a car shell, a heat sink of a computer device, a middle plate of a mobile phone, a mobile phone shell, a heat sink of an LED lamp, thin parts of 5G products, etc.
[0172] Embodiment 1
[0173] The aluminum source is heated at a temperature of 720° C. to obtain aluminum liquid;
[0174] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and B to the aluminum liquid, and keeping the temperature at 700° C. for 30 minutes to obtain an alloy liquid;
[0175] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of embodiment 1. In the aging treatment, the temperature of the first low-temperature aging treatment is -100°C and the time is 2h; the temperature of the second low-temperature aging treatment is 20°C and the time is 5h; the temperature of the third high-temperature aging treatment is 280°C and the time is 10h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si aluminum alloy contains Si with a mass percentage content of 5%, Fe with a mass percentage content of 0.4%, Cu with a mass percentage content of 0.001%, Mg with a mass percentage content of 0.001%, Sr with a mass percentage content of 0.005%, Zn with a mass percentage content of 0.001%, Ni with a mass percentage content of 0.01%, and B with a mass percentage content of 0.0008%.
[0176] Comparative Example 1
[0177] The aluminum source is heated at a temperature of 720° C. to obtain aluminum liquid;
[0178] Adding Si, Fe, Cu, Mg, Sr, Zn, and B to the aluminum liquid, and keeping the temperature at 700° C. for 30 minutes to obtain an alloy liquid;
[0179] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of comparative example 1. In the aging treatment, the temperature of the first low-temperature aging treatment is -150°C and the time is 2h; the temperature of the second low-temperature aging treatment is 20°C and the time is 5h; the temperature of the third high-temperature aging treatment is 280°C and the time is 10h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si aluminum alloy contains 5% Si by mass, 0.4% Fe by mass, 0.001% Cu by mass, 0.001% Mg by mass, 0.005% Sr by mass, 0.001% Zn by mass, and 0.0008% B by mass.
[0180] Comparative Example 2
[0181] The aluminum source is heated at a temperature of 720° C. to obtain aluminum liquid;
[0182] Adding Si, Fe, Cu, Mg, Sr, Zn, and B to the aluminum liquid, and keeping the temperature at 700° C. for 30 minutes to obtain an alloy liquid;
[0183] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of comparative example 2. In the aging treatment, the temperature is 250°C and the time is 6h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si aluminum alloy contains Si with a mass percentage content of 5%, Fe with a mass percentage content of 0.4%, Cu with a mass percentage content of 0.001%, Mg with a mass percentage content of 0.001%, Sr with a mass percentage content of 0.005%, Zn with a mass percentage content of 0.001%, and B with a mass percentage content of 0.0008%.
[0184] Embodiment 2
[0185] The aluminum source is heated at a temperature of 720° C. to obtain aluminum liquid, wherein the aluminum liquid contains Mn, Cr, Ti, and V;
[0186] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and B to the aluminum liquid, and keeping the temperature at 700° C. for 30 minutes to obtain an alloy liquid;
[0187] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of embodiment 1. The temperature of the aging treatment is 300°C and the time is 3h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si aluminum alloy contains 8% Si by mass, 0.4% Fe by mass, 0.05% Cu by mass, 0.05% Mg by mass, 0.04% Sr by mass, 0.1% Zn by mass, 0.2% Ni by mass, 0.01% B by mass, 0.005% Mn by mass, 0.003% Ti by mass, 0.004% Cr by mass, and 0.002% V by mass.
[0188] Embodiment 3
[0189] The aluminum source is heated at a temperature of 720° C. to obtain aluminum liquid, wherein the aluminum liquid contains Mn, Cr, Ti, and V;
[0190] Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, and B to the aluminum liquid, and keeping the temperature at 700° C. for 30 minutes to obtain an alloy liquid;
[0191] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of Example 1. In the aging treatment, the temperature of the first low-temperature aging treatment is -110°C and the time is 1 hour; the temperature of the second low-temperature aging treatment is 25°C and the time is 2 hours; the temperature of the third high-temperature aging treatment is 310°C and the time is 1 hour. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5 m / s. The Al-Si aluminum alloy contains 5.2% Si by mass, 0.8% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.02% Sr by mass, 0.008% Zn by mass, 0.03% Ni by mass, 0.001% B by mass, 0.005% Mn by mass, 0.006% Ti by mass, 0.005% Cr by mass, and 0.005% V by mass.
[0192] Embodiment 4
[0193] The aluminum source is heated at a temperature of 750° C. to obtain aluminum liquid, wherein the aluminum liquid contains Mn, Cr, Ti, and V;
[0194] Adding Si, Fe, Cu, Mg, Sr, Zn, Co, Cd, RE, Ni, and B to the aluminum liquid, and keeping the temperature at 720° C. for 10 minutes to obtain an alloy liquid;
[0195] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of Example 4. In the aging treatment, the temperature of the first low-temperature aging treatment is -150°C and the time is 5h; the temperature of the second low-temperature aging treatment is 40°C and the time is 10h; the temperature of the third high-temperature aging treatment is 310°C and the time is 12h. The alloy liquid is subjected to die casting treatment at a temperature of 660°C, wherein the die casting speed of the die casting machine is 0.5m / s. The Al-Si aluminum alloy contains 5.2% Si by mass, 0.8% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.02% Sr by mass, 0.008% Zn by mass, 0.03% Ni by mass, 0.001% B by mass, 0.005% Mn by mass, 0.006% Ti by mass, 0.005% Cr by mass, 0.005% V by mass, 0.05% Co by mass, 0.005% Cd by mass, and 0.01% RE by mass.
[0196] Embodiment 5
[0197] The aluminum source is heated at a temperature of 760° C. to obtain aluminum liquid, wherein the aluminum liquid contains Mn, Cr, Ti, and V;
[0198] Add Si, Fe, Cu, Mg, Sr, Zn, Sn, Te, Be, Co, Ni, and B to the aluminum liquid, and keep the temperature at 720° C. for 20 minutes to obtain an alloy liquid;
[0199] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of Example 5. In the aging treatment, the temperature of the first low-temperature aging treatment is -200°C and the time is 10h; the temperature of the second low-temperature aging treatment is 70°C and the time is 1h; the temperature of the third high-temperature aging treatment is 350°C and the time is 0.1h. The alloy liquid is subjected to die casting treatment at a temperature of 680°C, wherein the die casting speed of the die casting machine is 1m / s. The Al-Si aluminum alloy contains 5% Si by mass, 0.8% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.02% Sr by mass, 0.008% Zn by mass, 0.03% Ni by mass, 0.001% B by mass, 0.005% Mn by mass, 0.006% Ti by mass, 0.005% Cr by mass, 0.005% V by mass, 0.003% Sn by mass, 0.003% Te by mass, 0.006% Be by mass, and 0.02% Co by mass.
[0200] Embodiment 6
[0201] The aluminum source is heated at a temperature of 770° C. to obtain aluminum liquid, wherein the aluminum liquid contains Mn, Cr, Ti, and V;
[0202] Add Si, Fe, Cu, Mg, Sr, Zn, Sn, In, Nb, Bi, Ge, Mo, Ag, Ni, and B to the aluminum liquid, and keep the temperature at 750° C. for 150 minutes to obtain an alloy liquid;
[0203] After the alloy liquid is subjected to refining treatment and slag removal treatment, it is subjected to die casting treatment and aging treatment to obtain the Al-Si aluminum alloy of Example 6. In the aging treatment, the temperature of the first-level low-temperature aging treatment is 100°C and the time is 1 hour; the temperature of the second-level low-temperature aging treatment is 60°C and the time is 1 hour; the temperature of the third-level high-temperature aging treatment is 340°C and the time is 5 hours. The alloy liquid is subjected to die casting treatment at a temperature of 670°C, wherein the die casting speed of the die casting machine is 1.5 m / s. The Al-Si aluminum alloy contains 5% Si by mass, 0.8% Fe by mass, 0.005% Cu by mass, 0.005% Mg by mass, 0.02% Sr by mass, 0.008% Zn by mass, 0.03% Ni by mass, 0.001% B by mass, 0.005% Mn by mass, and 0.01% Mn by mass. 0.006% Ti, 0.005% Cr, 0.005% V, 0.01% Sn, 0.002% In, 0.002% Nb, 0.0001% Bi, 0.005% Ge, 0.001% Mo, and 0.0002% Ag.
[0204] Table 1 Performance test results of Examples 1 to 6 and Comparative Examples 1 to 2
[0205] Group Yield strength(MPa) Elongation(%) Thermal conductivity (w / mk) Embodiment 1 122 17.2 208 Embodiment 2 125 17.6 212 Embodiment 3 127 18.1 209 Embodiment 4 131 16.8 201 Embodiment 5 128 16.7 214 Embodiment 6 133 16.1 207 Comparative Example 1 106 14.2 182 Comparative Example 2 103 14.6 189
[0206] According to Table 1, the yield strength, elongation, and electrical conductivity of the Al-Si aluminum alloys of Examples 1 to 6 are better than those of the Al-Si aluminum alloys of Comparative Examples 1 to 2. Moreover, the Al-Si aluminum alloys of Examples 1 to 6 can simultaneously meet the following requirements: thermal conductivity greater than 200, yield strength greater than 120 MPa, and elongation greater than 16%, and have great market application prospects.
[0207] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. An Al-Si aluminum alloy containing aluminum, characterized in that: The Al-Si series aluminum alloy further contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.09% Ni by mass, 0.0008-0.01% B by mass, 0.0001-0.004% Mn by mass, 0.0001-0.008% Ti by mass, 0.0001-0.008% Cr by mass, 0.0001-0.008% V by mass, and 0.0001-0.008% C by mass. The Al-Si series aluminum alloy has a thermal conductivity greater than 200 W / m·k and an elongation greater than 16%. The Al-Si series aluminum alloy is subjected to aging treatment, and the aging treatment includes a primary low-temperature aging treatment, a secondary low-temperature aging treatment and a tertiary high-temperature aging treatment. The temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1h to 15h. The temperature of the secondary low-temperature aging treatment is 0°C to 70°C, and the time is 1h to 24h. The temperature of the tertiary high-temperature aging treatment is 280°C to 350°C, and the time is 0.05h to 15h.
2. The Al-Si aluminum alloy according to claim 1, characterized in that: The Al-Si aluminum alloy contains 6-7.5% Si by mass, 0.5-0.7% Fe by mass, 0.005-0.04% Cu by mass, 0.003-0.04% Mg by mass, 0.01-0.02% Sr by mass, 0.008-0.05% Zn by mass, 0.01-0.028% Ni by mass, and 0.005-0.01% Cu by mass. The content of B is 0.0009-0.01% by mass, the content of Mn is 0.001-0.004% by mass, the content of Ti is 0.001-0.008% by mass, the content of Cr is 0.001-0.008% by mass, the content of V is 0.001-0.008% by mass, the content of RE is 0.001-0.02% by mass, and the content of Nb is 0.0001-0.005% by mass.
3. The Al-Si aluminum alloy according to claim 1, characterized in that: Meet at least one of the following conditions: The mass ratio of Si to Fe is 5-20:1; The mass ratio of Ni to Nb is 1-50:1; The mass ratio of Si to Sr is 200-1500:1; The mass ratio of Mg, Cu, and Zn is 0.1-1:0.1-1:1; The sum of the mass percentages of Cu, Mg, Zn, and B shall not exceed 0.2%; The sum of the mass percentage contents of Si, Fe, Cu, Mg, Sr, Zn, Ni, and B is not more than 9%.
4. The Al-Si aluminum alloy according to any one of claims 1 to 3, characterized in that: Meet at least one of the following conditions: The Al-Si aluminum alloy further contains 0-0.009% by mass of In; The Al-Si aluminum alloy further contains Bi in an amount of 0-0.006% by mass; The Al-Si aluminum alloy further contains Ge in an amount of 0-0.005% by mass; The Al-Si aluminum alloy further contains 0-0.005% by mass of Mo; The Al-Si aluminum alloy further contains Ag in an amount of 0-0.005% by mass; The Al-Si aluminum alloy further contains Sn in an amount of 0-0.1% by mass; The Al-Si aluminum alloy further contains Te in an amount of 0-0.005% by mass; The Al-Si aluminum alloy further contains 0-0.01% Be by mass percentage; The Al-Si aluminum alloy further contains Co in an amount of 0-0.1% by mass; The Al-Si aluminum alloy further contains Cd in an amount of 0-0.01% by mass; RE is at least one of La, Ce, Pr, Nd, Er, Sm, Y, and Gd.
5. The Al-Si aluminum alloy according to claim 4, characterized in that: Meet at least one of the following conditions: When the Al-Si aluminum alloy contains In, the mass ratio of Cu to In is 0.1-20:1; When the Al-Si aluminum alloy contains Bi, the mass ratio of Mg to Bi is 10-450:1; When the Al-Si aluminum alloy contains Ge, the mass ratio of Si to Ge is 1000-2000:1; When the Al-Si aluminum alloy contains Mo, the mass ratio of Si to Mo is 1500-2000:1; When the Al-Si aluminum alloy contains Ag, the mass ratio of Mg to Ag is 10-500:1, and the mass ratio of Cu to Ag is 10-400:1; When the Al-Si aluminum alloy contains Sn and Te, the mass ratio of Mg to Sn is 0.3-10:1, and the mass ratio of Te to Sn is 0.01-1:1; When the Al-Si aluminum alloy contains Be and Co, the mass ratio of Be, Co, and Fe is 0.001-0.03:0.004-0.25:1, and the mass ratio of Fe and Co is 1-250:1; When the Al-Si aluminum alloy contains Be and Cd, the mass ratio of RE, Sr and Fe is 0.002-0.1:0.02-0.08:1, the mass ratio of RE, B and Fe is 0.002-0.1:0.0001-0.03:1, the mass ratio of RE and Cd is 0.1-25:1, and the mass ratio of RE, B and Be is 0.5-20:0.1-10:
1.
6. The Al-Si aluminum alloy according to claim 4, characterized in that: The Al-Si aluminum alloy also contains 0.0001-0.009% In by mass, 0.0001-0.006% Bi by mass, 0.0001-0.005% Ge by mass, 0.0001-0.005% Mo by mass, 0.0001-0.005% Ag by mass, 0.0001-0.005% Sn by mass, 0.0001-0.1% Te by mass, 0.0001-0.005% Be by mass, 0.001-0.01% Co by mass, and 0.001-0.008% Cd by mass.
7. A method for preparing the Al-Si aluminum alloy according to any one of claims 1 to 6, comprising the following steps: The aluminum source is subjected to a first heating treatment to obtain aluminum liquid; Adding Si, Fe, Cu, Mg, Sr, Zn, Ni, Nb, RE, and B to the aluminum liquid, performing a second heating treatment, and obtaining an alloy liquid; Refining and slagging the alloy liquid, and testing its composition and content; and After the composition and content are qualified, the alloy liquid after the refining treatment and the slag removal treatment is subjected to die casting treatment and aging treatment to obtain an Al-Si series aluminum alloy, wherein the Al-Si series aluminum alloy contains 5-8% Si by mass, 0.4-0.8% Fe by mass, 0.001-0.05% Cu by mass, 0.001-0.05% Mg by mass, 0.005-0.04% Sr by mass, 0.001-0.1% Zn by mass, 0.01-0.09% Ni by mass, 0.0008-0.01% B by mass, 0.0001-0.004% Mn by mass, 0.0001-0.008% Ti by mass, 0.0001-0.0 08% Cr, 0.0001-0.008% V, 0.001-0.02% RE, and 0.0001-0.005% Nb, wherein Mn, Ti, Cr, and V are impurities, and the sum of the mass percentages of Mn, Ti, Cr, and V is not more than 0.025%, and the aging treatment includes a primary low-temperature aging treatment, a secondary low-temperature aging treatment, and a tertiary high-temperature aging treatment, wherein the temperature of the primary low-temperature aging treatment is -100°C to -200°C, and the time is 1h to 15h; the temperature of the secondary low-temperature aging treatment is 0°C to 70°C, and the time is 1h to 24h; the temperature of the tertiary high-temperature aging treatment is 280°C to 350°C, and the time is 0.05h to 15h, and the thermal conductivity of the Al-Si series aluminum alloy is greater than 200W / m·k, and the elongation is greater than 16%.
8. The method for preparing the Al-Si series aluminum alloy according to claim 7, characterized in that: The aluminum source is at least one of original aluminum, aluminum ingot, and recycled aluminum; The preparation method of the Al-Si aluminum alloy also includes the step of adding at least one of In, Bi, Ge, Mo, Ag, Sn, Te, Be, Co, and Cd to the aluminum liquid.
9. A heat dissipation structure, characterized in that: At least part of the heat dissipation structure is made of the Al-Si series aluminum alloy described in any one of claims 1-6 or the Al-Si series aluminum alloy prepared by the preparation method of the Al-Si series aluminum alloy described in any one of claims 7-8.
Citation Information
Patent Citations
Aluminum alloy and application thereof
CN112159916A
Aluminum alloy with high thermal conductivity and preparation method thereof
CN113005341A
Aluminum alloy, die casting, electronic equipment and preparation method of aluminum alloy
CN115109971A
Aluminum alloys with grain refiners, and methods of making and using same
CN117144196A
Al-Mg-Si-Sn-RE series rare earth aluminum alloy, preparation method thereof and heat-resistant cable