A test method and device for testing reinforced concrete

Through the combination of seawater corrosion, air-drying irradiation and falling hammer impact test, the corrosion and impact performance of reinforced concrete in marine environment was simulated, and the problem that the existing technology could not effectively detect the reinforced concrete structure in marine environment is solved, and the reinforced concrete was realized. More accurate evaluation and screening.

CN118032626BActive Publication Date: 2024-11-22HEBEI XINDA IRON & STEEL GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311835331.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-11-22
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

The prior art cannot effectively simulate the corrosion and impact resistance of reinforced concrete structures in marine environments, especially the influence of dry and wet seawater and sunlight irradiation, resulting in detection lag behind structural research and development requirements.

Method used

Using a combination of seawater corrosion test, air-drying irradiation test and hammer impact test, a comprehensive evaluation of reinforced concrete samples was carried out by simulating corrosion conditions in the marine environment, including the use of laminar flow simulator to simulate seawater laminar flow, ultraviolet lamp and incandescent lamp simulation Sunlight exposure, as well as steel ball impact test simulates free-fall hammer impact.

Benefits of technology

Effectively accelerate the corrosion process of reinforced concrete in marine environments, simulate the erosion effect of sea breeze and sunlight, and evaluate its impact resistance through free-fall hammer impact test, screen out the types of reinforced concrete suitable for marine environments, and improve the detection Accuracy and applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118032626B_ABST
    Figure CN118032626B_ABST
Patent Text Reader

Abstract

This patent provides a test method and device for testing reinforced concrete, which relates to the field of material simulation test technology, including using seawater with specific required components to simulate the comprehensive marine environment such as dry-wet alternating corrosion, sunlight and sea breeze weathering erosion, etc. on reinforced concrete, and then performing a drop hammer impact test on the corroded reinforced concrete and evaluating the test results; it also includes seawater corrosion test devices, air-drying irradiation test devices, and drop hammer impact test devices used in the simulation test. This patent adopts a test method for testing reinforced concrete and the device used in the method to more realistically and comprehensively simulate the corrosion damage of reinforced concrete structures by seawater with specific components in a comprehensive marine environment, and classifies and rates the tested reinforced concrete through testing and evaluation of the test results, so as to screen out reinforced concrete that is more suitable for use in the marine environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material simulation testing, and in particular to a test method and a use device for testing reinforced concrete. Background Art

[0002] Steel bar corrosion is one of the reasons for the premature failure and destruction of concrete structures. Corrosion, especially the corrosion of steel bars in concrete, is one of the leading and key factors affecting the durability of the entire structure. Reinforced concrete structures located in the marine environment are corroded by high concentrations of corrosive ions for a long time, and the effects of wave loads, dry-wet alternation and other factors have led to prominent steel bar corrosion, which seriously affects the service life of the entire structure.

[0003] The individual or combined effects of chloride, freeze-thaw, carbonation, sulfate and alkali aggregate not only cause damage to the structural concrete body, but also induce corrosion of the steel bars in the concrete, leading to cracking and spalling of the structural concrete protective layer, reduction in steel bar cross-section, reduced bonding strength, and weakened bearing capacity, ultimately leading to the destruction of the reinforced concrete structure.

[0004] Safe operation and long service life are of great significance to resource conservation and sustainable development of society. At the same time, various tests on reinforced concrete structures are the prerequisite for sustainable research and development.

[0005] Existing technologies include: (1) Measuring crack width with the aid of a magnifying glass or naked eye: When the tensile stress caused by the expansion force of the steel bar corrosion exceeds the tensile strength of the concrete, cracks will appear in the concrete around the steel bar. The width of the crack is closely related to the degree of corrosion of the steel bar. (2) Drilling samples from the core of the reinforced concrete structure and testing under a press.

[0006] Existing detection and testing technologies have seriously lagged behind the development needs of reinforced concrete structures. They cannot simulate the ocean tidal range area where the structure will be submerged in seawater during high tide and exposed to the atmosphere during low tide, that is, the impact of the combined effects of periodic dry and wet changes with the tides and sunlight and sea breeze on reinforced concrete structures. Existing technologies do not solve the impact resistance and evaluation results of reinforced concrete structures after corrosion. Summary of the invention

[0007] In order to overcome the problem that the prior art cannot simulate the corrosion of reinforced concrete structures by alternating dry and wet conditions of seawater under laminar flow conditions, and that the prior art does not solve the problem of the impact resistance and evaluation results of reinforced concrete structures after corrosion, this patent provides a test method for reinforced concrete, including: conducting seawater corrosion tests, air-drying irradiation tests and drop hammer impact tests on samples, and evaluating the test results of the samples based on the light transmittance area and water seepage of the samples after the tests.

[0008] Preferably, the sample is first subjected to a seawater corrosion test and an air-drying irradiation test alternately, and then subjected to a drop weight impact test and evaluated based on the results of the drop weight impact test. The test time of the seawater corrosion test and the air-drying irradiation test are both 10 to 14 hours, and the sum of the test time of the seawater corrosion test and the air-drying irradiation test is 12 to 30 days.

[0009] Preferably, in the seawater corrosion test, an aerator is used to make the dissolved oxygen content of the seawater 5 to 10 mg / L, and a laminar flow device is used to make the seawater flow toward the sample at a flow rate of 0.3 to 1.0 m / s in a laminar flow state;

[0010] The air-drying irradiation test irradiates the sample with an ultraviolet lamp, heats the surface of the sample with an incandescent lamp, and atomizes the seawater and blows it toward the sample with an atomizer and a blower;

[0011] The power of the ultraviolet lamp is 15W, the number is 4 to 8, the surface temperature of the sample is 45 to 65° C., and the wind speed of the blower is 8 to 15 m / s.

[0012] Preferably, the pH value of the seawater used for the test is 7.2-8.6, the concentration of NaCl is 2%-5%, and the conductivity is 45×10 -3 ~50×10 -3 Ω·cm -1 , the temperature is 18 ~ 28℃.

[0013] Preferably, the sample is first placed in a sample freezer at 0 to -20°C for 2 to 8 hours, and then impacted 2 to 5 times with a steel ball, the mass of the steel ball being 15 to 20 kg, the diameter being 150 to 200 mm, and the distance between the steel ball and the sample being 1000 to 2000 mm.

[0014] Preferably, when the sample is light-transmitting, a light source is used to illuminate one side of the sample, and the maximum distance from the center to the edge of the transmission aperture is the radius r, and the light-transmitting area A=πr2 is calculated, and the sample to be tested with the light-transmitting area A=0 is evaluated as a sample of group A; the sample to be tested with the light-transmitting area A≠0 is evaluated as a sample of group B, and the samples of group B are sorted into B1, B2, B3, ..., Bn grades according to the light-transmitting areas of the samples from small to large;

[0015] When the sample is opaque, liquid is used to penetrate the sample. The volume of liquid is s. The time t for all the liquid to leak from the sample is recorded. The amount of water seepage per unit time Q = s / t. The samples in group A are divided into grades A1, A2, A3, ..., An according to the amount of water seepage per unit time Q from small to large.

[0016] A test device for testing reinforced concrete, including a seawater corrosion test device, an air-drying irradiation test device and a drop hammer impact test device:

[0017] The seawater corrosion testing device comprises a reaction tank, a laminar flow device is arranged above the reaction tank, the laminar flow device is connected to a water tank through a pipeline, and the water tank is installed above the laminar flow device through a bracket arranged on the bottom surface;

[0018] The air-drying irradiation testing device comprises a shell, a pair of clamping plates are arranged opposite to each other inside the shell, an irradiation mechanism is arranged near the inner wall of the shell, and an air-drying mechanism is arranged near the outer wall of the shell;

[0019] The drop hammer impact testing device comprises a safety cover, a steel ball capable of falling freely is arranged on the top of the safety cover, and an annular steel ring is arranged at the projection of the steel ball on the bottom of the safety cover.

[0020] Preferably, an aerator is provided in the water tank, the aerator is connected to the oxygen cylinder through a pipeline, and a pressure regulating station is provided on the pipeline between the aerator and the oxygen cylinder;

[0021] The storage tank is connected to the water tank through a pipeline, a pump is arranged on the pipeline between the storage tank and the water tank, and the storage tank is connected to the liquid distribution tank through a pipeline, a pump is arranged on the pipeline between the storage tank and the liquid distribution tank.

[0022] Preferably, the irradiation mechanism comprises an incandescent lamp and an ultraviolet lamp, and the incandescent lamp and the ultraviolet lamp are alternately arranged along the circumference of the inner wall of the shell;

[0023] The air drying mechanism comprises an atomizer, a blower and an air nozzle which are sequentially connected in series, and the air nozzle is arranged close to the inner wall of the shell.

[0024] Preferably, an expandable and retractable mechanical claw is provided at the top of the safety cover. When the mechanical claw is in a retracted state, there is a limiting space inside the mechanical claw. The steel ball is arranged in the limiting space of the mechanical claw. The annular steel ring is fixed on the steel plate embedded part. Anchor hooks are provided on the lower surface of the steel plate embedded part. The steel plate embedded parts are fixed in the concrete casting sand and gravel through the anchor hooks.

[0025] Compared with the prior art, the beneficial effects of this patent are:

[0026] 1. The present invention accelerates the simulation of seawater alternating corrosion, air-drying irradiation simulation and subsequent free-falling hammer impact test of reinforced concrete structures, which is conducive to the dry-wet alternation of cathode oxidation-reduction reaction during the corrosion process, so that a higher salt concentration is deposited on the surface of the area, accelerating the corrosion effect, and also simulating the state of reinforced concrete under the erosion of sea breeze and sunlight. After a series of comprehensive marine environment simulations and free-falling hammer impact, the reinforced concrete structure is evaluated for water penetration, and the types of reinforced concrete that are more suitable for use in marine environments can be screened out.

[0027] 2. The present application discloses a seawater corrosion device for testing reinforced concrete, including a water tank arranged at a high position. Under the action of gravity, the seawater stored in the water tank flows to the laminar flow meter, and after being redistributed by the laminar flow meter, the seawater flows in a laminar flow state to the test samples contained in the reaction tank below the laminar flow meter. This well simulates the corrosion of the test samples by seawater under the laminar flow state, and can simulate the natural marine environment, where seawater generates waves under the action of gravity, thereby producing alternating dry and wet corrosion effects on concrete structures in the marine environment.

[0028] 3. The present application discloses an air-drying irradiation device for testing reinforced concrete, which includes alternating ultraviolet lamps and incandescent lamps to simulate ultraviolet light and visible light in sunlight in a marine environment. While simulating sunlight, the main factors affecting corrosion in sunlight are taken into account, so as to more accurately simulate the effect of sunlight on corrosion of reinforced concrete in a marine environment.

[0029] 4. The present application discloses a drop hammer impact device for reinforced concrete testing, which uses a steel ball to perform impact tests on corroded reinforced concrete component samples, which can effectively solve the problem that the prior art cannot test large samples of reinforced concrete structures, and can well complete the impact resistance test of reinforced concrete structures after alternating seawater corrosion. By adjusting the weight, height and number of impacts of the steel ball, repeated tests can well achieve the purpose of the free drop hammer impact test. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of this patent or the technical solutions in the prior art, the following is a brief introduction to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of this patent. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a flow chart of the test method for testing reinforced concrete of this patent;

[0032] Figure 2This is a schematic diagram of the structure of the seawater corrosion testing device of this patent;

[0033] Figure 3 It is a schematic diagram of the side cross-section structure of the air-drying irradiation test device of this patent;

[0034] Figure 4 This is a schematic diagram of the top view of the air-drying irradiation test device of this patent;

[0035] Figure 5 This is a schematic diagram of the structure of the drop weight impact test device of this patent;

[0036] Among them: 1-reaction tank, 2-bracket, 3-water tank, 4-laminar flow device, 5-aerator, 6-pipeline, 7-pressure regulating station, 8-oxygen cylinder, 9-storage tank, 10-liquid distribution box, 11-pump, 12-housing, 13-incandescent lamp, 14-ultraviolet lamp, 15-atomizer, 16-fan, 17-nozzle, 18-motor, 19-first splint, 20-second splint, 21-reducer, 22-drying barrel, 23-fixed support, 24-adjustment plate, 25-adjustment shaft, 26-base, 27-steel ball, 28-lifting ear, 29-mechanical claw, 30-tightening spring, 31-electromagnetic switch, 32-safety cover, 33-corroded reinforced concrete component sample, 34-annular steel ring, 35-steel plate embedded parts, 36-anchor hook, 37-concrete casting sand and gravel. DETAILED DESCRIPTION

[0037] The following will be combined with specific embodiments to clearly and completely describe the technical solution of this patent. Obviously, the described embodiments are only part of the embodiments of this patent, not all of them. Based on the embodiments in this patent, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this patent.

[0038] In the field of simulation of reinforced concrete in marine environment, the existing detection and testing technology has seriously lagged behind the speed of research and development of reinforced concrete structures. It cannot simulate the influence of the periodic dry-wet alternation with the tides in the marine tidal range area, where the reinforced concrete structure will be submerged in seawater during high tide and exposed to the atmosphere during low tide, and the reinforced concrete structure will be subjected to a series of comprehensive environmental simulations such as seawater corrosion and wind drying before being subjected to a drop hammer impact test. The existing technology does not solve the impact resistance and evaluation results of reinforced concrete structures after corrosion.

[0039] When faced with the above problems, the solution usually adopted by those skilled in the art is to optimize one of the test methods and devices used in seawater corrosion simulation, air-drying irradiation test or drop hammer impact test, aiming to more accurately simulate the reinforced concrete in one of the tests and obtain more accurate data.

[0040] After long-term experiments and summaries, the inventor of this patent provides a test method and device for testing reinforced concrete. Through the cooperation of seawater corrosion test device, air-drying irradiation test device and drop hammer impact test device, the corrosion of reinforced concrete in a comprehensive marine environment is simulated, and the evaluation method of drop hammer impact test is used to evaluate the tested reinforced concrete sample. The specific technical solution is as follows:

[0041] Reference Figure 1 A test method for testing reinforced concrete, comprising: performing seawater corrosion test, air-drying irradiation test and drop hammer impact test on the sample, and evaluating the test results of the sample according to the light transmission area and water seepage of the sample after the test.

[0042] Specifically, the samples are first subjected to alternate seawater corrosion tests and air-drying irradiation tests, and then subjected to drop weight impact tests and evaluated based on the results of the drop weight impact tests. The test times of the seawater corrosion test and the air-drying irradiation test are both 10 to 14 hours, and the sum of the test times of the seawater corrosion test and the air-drying irradiation is 12 to 30 days.

[0043] Specifically, in the seawater corrosion test, the dissolved oxygen content of the seawater is 5 to 10 mg / L using an aerator 5, and the seawater is made to flow toward the sample at a flow rate of 0.3 to 1.0 m / s in a laminar flow state using a laminar flow device 4;

[0044] The air-drying irradiation test uses an ultraviolet lamp 14 to irradiate the sample, uses an incandescent lamp 13 to heat the surface of the sample, and uses an atomizer 15 and a blower 16 to atomize the seawater and blow it toward the sample;

[0045] The power of the ultraviolet lamp 14 is 15W, the number is 4 to 8, the surface temperature of the sample is 45 to 65° C., and the wind speed of the blower 16 is 8 to 15 m / s.

[0046] Specifically, the pH value of the seawater used for the test is 7.2-8.6, the concentration of NaCl is 2%-5%, the conductivity is 45×10-3-50×10-3Ω·cm-1, and the temperature is 18-28°C.

[0047] Specifically, the sample is first placed in a sample freezer at 0 to -20°C for 2 to 8 hours, and then impacted 2 to 5 times by a steel ball 27, wherein the mass of the steel ball 27 is 15 to 20 kg, the diameter is 150 to 200 mm, and the distance between the steel ball 27 and the sample is 1000 to 2000 mm.

[0048] Specifically, when the sample is light-transmitting, a light source is used to illuminate one side of the sample, and the maximum distance from the center to the edge of the transmission aperture is the radius r, and the light-transmitting area A=πr2 is calculated. The sample to be tested with the light-transmitting area A=0 is evaluated as a sample of group A; the sample to be tested with the light-transmitting area A≠0 is evaluated as a sample of group B, and the samples of group B are sorted into B1, B2, B3, ..., Bn levels according to the light-transmitting areas of the samples from small to large;

[0049] When the sample is opaque, liquid is used to penetrate the sample. The volume of liquid is s. The time t for all the liquid to leak from the sample is recorded. The amount of water seepage per unit time Q = s / t. The samples in group A are divided into grades A1, A2, A3, ..., An according to the amount of water seepage per unit time Q from small to large.

[0050] Reference shown Figures 2 to 5 , a test device for testing reinforced concrete, including a seawater corrosion test device, an air-drying irradiation test device and a drop hammer impact test device:

[0051] The seawater corrosion testing device comprises a reaction tank 1, a laminar flow device 4 is arranged above the reaction tank 1, the laminar flow device 4 is connected to a water tank 3 through a pipeline 6, and the water tank 3 is installed above the laminar flow device 4 through a bracket 2 arranged on the bottom surface;

[0052] The air-drying irradiation testing device comprises a housing 12, a pair of clamping plates are arranged opposite to each other inside the housing 12, an irradiation mechanism is arranged near the inner wall of the housing 12, and an air-drying mechanism is arranged near the outer wall of the housing 12;

[0053] The drop hammer impact test device comprises a safety cover 32 , a steel ball 27 which can fall freely is arranged on the top of the safety cover 32 , and an annular steel ring 34 is arranged at the projection of the steel ball 27 on the bottom of the safety cover 32 .

[0054] Specifically, an aerator 5 is provided in the water tank 3, and the aerator 5 is connected to an oxygen cylinder 8 through a pipeline 6, and a pressure regulating station 7 is provided on the pipeline 6 between the aerator 5 and the oxygen cylinder 8;

[0055] The storage tank 9 is connected to the water tank 3 through a pipeline 6, and a pump 11 is provided on the pipeline 6 between the storage tank 9 and the water tank 3. The storage tank 9 is connected to the liquid distribution tank 10 through a pipeline 6, and a pump 11 is provided on the pipeline 6 between the storage tank 9 and the liquid distribution tank 10.

[0056] Specifically, the irradiation mechanism includes an incandescent lamp 13 and an ultraviolet lamp 14, and the incandescent lamp 13 and the ultraviolet lamp 14 are alternately arranged along the inner wall of the housing 12 to simulate the irradiation effect of sunlight on the corrosion of reinforced concrete;

[0057] The air-drying mechanism comprises an atomizer 15, a fan 16 and an air nozzle 17 which are sequentially connected in series. The air nozzle 17 is arranged close to the inner wall of the housing 12 to simulate the corrosive effect of sea breeze on reinforced concrete.

[0058] Specifically, the housing 12 is made of stainless steel, and the inner wall of the housing 12 is polished to reflect light and enhance the lighting efficiency of the irradiation mechanism.

[0059] In order to make each test surface of the reinforced concrete member corrode to the same extent, the present embodiment is further provided with a motor 18, a second clamping plate 2019 relatively arranged inside the housing 12, and a second clamping plate;

[0060] A hollow base 26 is provided below the housing 12, the motor 18 is provided inside the base 26 and the output shaft passes through the housing 12; the second clamping plate 2019 and the second clamping plate are arranged opposite to each other and leave a gap for placing reinforced concrete components, the second clamping plate 2019 is connected to the output shaft of the motor 18 on one side away from the second clamping plate, and a reducer 21 is provided between the output end of the motor 18 and the second clamping plate 2019, at this time, the output end axis of the reducer 21 is the output shaft of the motor 18, which can increase the torque and reduce the loss of the motor 18;

[0061] The second clamping plate is rotatably connected to the housing 12 on one side away from the second clamping plate 2019. When air-drying and irradiation is performed, the reinforced concrete component is fixed in the second clamping plate 2019 and the second clamping plate, and the motor 18 drives the reinforced concrete component to rotate, so that the reinforced concrete component is evenly irradiated by the ultraviolet lamp 14, the incandescent lamp 13, and the liquid mist is sprayed at the air nozzle 17;

[0062] At the same time, the air nozzles 17 are evenly arranged circumferentially around the output shaft of the motor 18, and the spraying direction is toward the reinforced concrete component, so that the sprayed liquid mist is evenly distributed around the reinforced concrete component.

[0063] A drying barrel 22 is provided along the inner wall of the outer shell 12. During the rotation of the reinforced concrete component, the excess water on the reinforced concrete component is separated by the centrifugal force and reaches the inner wall of the drying barrel 22, and then gathers downward along the inner wall of the drying barrel 22 to be discharged. When the experiment is finished, the speed of the motor 18 is increased to quickly dry the water on the reinforced concrete component so as to quickly start the subsequent experiment.

[0064] A fixed support 23 is provided on the outside of the outer shell 12, and an adjustment plate 24 is slidably provided on the fixed support 23. An adjustment shaft 25 is provided in the center of the adjustment plate 24. One end of the adjustment shaft 25 passes through the outer shell 12 and is rotatably connected to the adjustment plate 24 through a bearing, and a baffle is provided at the end. The other end of the adjustment shaft 25 is fixedly connected to the second clamping plate.

[0065] As an easily conceivable implementation of the "sliding setting", it can be a sliding rod and sliding sleeve that cooperate with each other. Specifically, a groove along the sliding direction is provided on the fixed support 23, a sliding rod along the sliding direction is provided in the groove, and a sliding sleeve is fixedly connected to one end of the adjustment plate 24, and the sliding sleeve is set on the sliding rod.

[0066] The adjustment shaft 25 is colinear with the output shaft of the motor 18, and the sliding direction of the adjustment plate 24 is parallel to the adjustment shaft 25. The adjustment plate 24 can drive the second clamping plate to slide up and down to adjust the gap length between the second clamping plate 2019 and the second clamping plate to meet the experimental needs of reinforced concrete components of various specifications.

[0067] Specifically, the top of the safety cover 32 is provided with an expandable and retractable mechanical claw 29. When the mechanical claw 29 is in a retracted state, there is a limited space inside the mechanical claw 29. The steel ball 27 is arranged in the limited space of the mechanical claw 29. The annular steel ring 34 is fixed on the steel plate embedded part 35. The lower surface of the steel plate embedded part 35 is provided with an anchor hook 36. The steel plate embedded part 35 is fixed in the concrete casting sand and gravel through the anchor hook 36. The annular steel ring 34 plays a role of fixing and supporting the corroded reinforced concrete component sample 33. The steel plate embedded part 35 buried in the concrete casting sand and gravel 37 and the anchor hook 36 fixed on its lower surface also play a role of supporting the corroded reinforced concrete component sample 33.

[0068] Specifically, the steel ball 27 is partially installed in the safety cover 32, the width of the upper part of the safety cover 32 is greater than the outer diameter of the steel ball 27, and the width of the upper opening of the safety cover 32 is matched with the outer diameter clearance of the steel ball 27 to accommodate the smooth falling of the steel ball 27 in the safety cover 32 and to constitute a closed environment for the free fall hammer impact test.

[0069] Using the steel ball 27 to carry out the impact test on the corroded reinforced concrete component sample 33 can effectively solve the problem that the prior art cannot test large samples of reinforced concrete structures, and can well complete the impact resistance test of reinforced concrete structures after alternating seawater corrosion. By adjusting the weight, height and number of impacts of the steel ball 27, repeated tests can well achieve the purpose of the free fall hammer impact test; when the steel ball 27 is tested, it is easy to roll randomly after falling, thereby injuring the staff, and the use of the safety cover 32 can form a barrier during the test work, allowing the steel ball 27 to fall smoothly inside it, which can effectively protect the physical safety of the staff.

[0070] Specifically, a lifting ear 28 and a mechanical claw 29 control component for grabbing or releasing the lifting ear 28 are fixedly connected above the steel ball 27, which is more conducive to the release of the steel ball 27 by the mechanical claw 29 and avoids the situation where the mechanical claw 29 is not fully deployed, resulting in difficulty in releasing the steel ball 27.

[0071] Specifically, a control unit is provided on the control assembly of the mechanical claw 29, and the control unit includes a tightening spring 30 and an electromagnetic switch 31. The mechanical claw 29 includes two openable and closable claw arms, and the two ends of the tightening spring 30 are respectively fixed on the two claw arms of the mechanical claw 29, so as to better control the opening and closing of the mechanical claw 29.

[0072] The above further describes this patent with the help of specific embodiments, but it should be understood that the specific description here should not be construed as a limitation on the essence and scope of this patent. Various modifications made to the above embodiments by ordinary technicians in this field after reading this specification are all within the scope of protection of this patent.

Claims

1. A test method for testing reinforced concrete, characterized in that: include: First, alternately subjecting the sample to a seawater corrosion test and an air-drying irradiation test, and then subjecting the sample to a drop weight impact test and evaluating the sample according to the results of the drop weight impact test; When the sample is transparent, a light source is used to illuminate one side of the sample, and the maximum distance from the center to the edge of the transmission aperture is taken as the radius r, and the transparent area A=πr is calculated. 2 , the samples with the light transmission area A=0 are evaluated as group A samples; the samples with the light transmission area A≠0 are evaluated as group B samples, and the group B samples are ranked into B1, B2, B3, ..., Bn grades according to the light transmission areas of the samples from small to large; When the sample is opaque, liquid is used to penetrate the sample. The volume of the liquid is s. The time t for all the liquid to leak from the sample is recorded. The amount of water seepage per unit time Q=s / t. The samples in group A are divided into grades A1, A2, A3, ..., An according to the amount of water seepage per unit time Q from small to large.

2. A test method for testing reinforced concrete according to claim 1, characterized in that: The test time of the seawater corrosion test and the air-drying irradiation test are both 10 to 14 hours, and the sum of the test time of the seawater corrosion test and the air-drying irradiation test is 12 to 30 days.

3. A test method for testing reinforced concrete according to claim 1, characterized in that: The seawater corrosion test uses an aerator to make the dissolved oxygen content of the seawater 5-10 mg / L, and uses a laminar flow device to make the seawater flow toward the sample at a flow rate of 0.3-1.0 m / s in a laminar flow state; The air-drying irradiation test irradiates the sample with an ultraviolet lamp, heats the surface of the sample with an incandescent lamp, and atomizes the seawater and blows it toward the sample with an atomizer and a blower; The power of the ultraviolet lamp is 15W, the number is 4 to 8, the surface temperature of the sample is 45 to 65° C., and the wind speed of the blower is 8 to 15 m / s.

4. A test method for testing reinforced concrete according to claim 3, characterized in that: The pH value of the seawater used for the test was 7.2-8.6, the concentration of NaCl was 2%-5%, and the conductivity was 45×10 -3 ~50×10 -3 Ω·cm -1 , the temperature is 18~28℃.

5. A test method for testing reinforced concrete according to claim 1, characterized in that: First, the sample is placed in a sample freezer at -20~0°C for 2~8h, and then impacted 2~5 times with a steel ball, the mass of which is 15~20kg and the diameter is 150~200mm, and the distance between the steel ball and the sample is 1000~2000mm.

6. The device used in the test method for testing reinforced concrete according to any one of claims 1 to 5, characterized in that: Including seawater corrosion test device, air drying irradiation test device and drop hammer impact test device: The seawater corrosion testing device comprises a reaction tank, a laminar flow device is arranged above the reaction tank, the laminar flow device is connected to a water tank through a pipeline, and the water tank is installed above the laminar flow device through a bracket arranged on the bottom surface; The air-drying irradiation testing device comprises a shell, a pair of clamping plates are arranged opposite to each other inside the shell, an irradiation mechanism is arranged near the inner wall of the shell, and an air-drying mechanism is arranged near the outer wall of the shell; The drop hammer impact testing device comprises a safety cover, a steel ball capable of falling freely is arranged on the top of the safety cover, and an annular steel ring is arranged at the projection of the steel ball on the bottom of the safety cover.

7. The device used in the test method for testing reinforced concrete according to claim 6, characterized in that: An aerator is arranged in the water tank, the aerator is connected to the oxygen cylinder through the pipeline, and a pressure regulating station is arranged on the pipeline between the aerator and the oxygen cylinder; The storage tank is connected to the water tank through the pipeline, a pump is arranged on the pipeline between the storage tank and the water tank, and the storage tank is connected to the liquid distribution tank through the pipeline, and the pump is arranged on the pipeline between the storage tank and the liquid distribution tank.

8. The device used in the test method for testing reinforced concrete according to claim 6, characterized in that: The irradiation mechanism includes an incandescent lamp and an ultraviolet lamp, and the incandescent lamp and the ultraviolet lamp are alternately arranged along the circumference of the inner wall of the shell; The air-drying mechanism comprises an atomizer, a blower and an air nozzle which are sequentially connected in series, and the air nozzle is arranged close to the inner wall of the shell.

9. The device used in the test method for testing reinforced concrete according to claim 6, characterized in that: The top of the safety cover is provided with an expandable and retractable mechanical claw. When the mechanical claw is in a retracted state, there is a limiting space inside the mechanical claw. The steel ball is arranged in the limiting space of the mechanical claw. The annular steel ring is fixed on the steel plate embedded part. The lower surface of the steel plate embedded part is provided with an anchor hook. The steel plate embedded part is fixed in the concrete casting sand and gravel through the anchor hook.

Citation Information

Patent Citations

  • Method for testing bump-milling resistance performance of ship lock concrete

    CN101251459A

  • Multi-factor interactive corrosion experiment device and method for simulating marine service environment

    CN111398150A

  • Corrosion simulation test device for reinforced concrete composite material