A friction catalyst for reducing CO2 and its preparation method and application

By using a heterostructure catalyst formed by tungsten bronze and zinc oxide, the problems of low CO2 reduction efficiency and environmental hazards in the existing technology are solved, efficient CO2 reduction and temperature stability are achieved, and the application prospects of tribocatalytic materials are expanded.

CN118059879BActive Publication Date: 2024-10-15GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410194205.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-10-15
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

In terms of CO2 reduction, the existing technology has problems such as low utilization of sunlight, being affected by light transmittance, and being unresponsive under no-light or low-light conditions. The reduction ability of tribocatalysts has not yet reached a satisfactory level, and traditional catalysts have harmful effects on the environment and human body. Potential hazards.

Method used

The heterostructure Ba0.75Sr0.25Nb1.9Ta0.1O6@ZnO formed by tungsten bronze material and zinc oxide is used as a tribocatalyst. Submicron powder materials are formed through specific preparation methods to reduce the use of lead-based ceramics and expand tribocatalytic materials. structure type.

Benefits of technology

It achieves efficient CO2 reduction, generating 274ppm CO within 12 hours. It has good temperature stability, simple process, reduces harm to the environment and human body, and has good industrialization prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118059879B_ABST
    Figure CN118059879B_ABST
Patent Text Reader

Abstract

The present invention discloses a friction catalyst for reducing CO2 and its preparation method and application, belonging to the field of energy and environmental treatment technology. The catalyst is a heterogeneous structure, and the chemical expression is Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O6@ZnO. The present invention uses BaCO3, SrCO3, Nb2O5, and Ta2O5 as raw materials, and after pressing and pre-sintering, successively carries out ball milling, drying, pressing, cold isostatic pressing, and sintering to obtain Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O6; then add ZnO solution for ultrasonication and stirring, filter and collect sediment, and then sinter to obtain the friction catalyst for reducing CO2. The friction catalyst provided by the present invention has good cycle stability, simple preparation method, significant CO2 reduction effect, and good industrialization prospect and application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energy and environmental treatment, and specifically relates to a method for reducing CO 2 Friction catalyst and preparation method and application thereof. Background Art

[0002] Energy and environmental issues are two major challenges that hinder the sustainable development of human society. In the past few decades, the continuous consumption of fossil fuels has led to energy shortages and the 2 The global greenhouse effect caused by emissions is becoming more and more serious, causing irreversible damage to the environment on which we depend for survival. 2 Reduction to CO is particularly important.

[0003] Among the many technologies for developing and utilizing clean energy, photocatalytic technology has the characteristics of sufficient energy source, clean process and low cost. It has been deeply studied and widely used in environmental governance, relieving energy pressure and reducing greenhouse gas emissions. For example, semiconductor nanomaterials are excited by sunlight to produce photogenerated electron-hole pairs with reactive activity. Water molecules or CO on their surface 2 Capturing photogenerated electrons and reducing them into hydrogen or chemical fuels such as methane, methanol, and carbon monoxide, also known as photolysis of water and CO 2 Photocatalytic reduction technology has significant advantages such as low energy consumption, low cost, and no pollution. However, photocatalytic technology has disadvantages such as low utilization of sunlight, being affected by light transmittance, and no response under no light or weak light conditions. The development and utilization of other forms of clean energy are now gaining more and more attention. Similarly, piezoelectric catalysis must achieve reaction conditions through high-frequency ultrasonic vibration, so it is challenging to implement in the natural environment. Therefore, the development of photocatalytic reduction technology for CO 2 New catalytic technologies for reduction to CO are particularly important.

[0004] Tribocatalysis belongs to the category of mechanical energy-electrical energy-catalysis. It realizes charge transfer at the solid / solid interface or liquid / solid interface through the triboelectrification effect, and forms a local electric field and polarization phenomenon. The positive and negative charges generated by friction can combine with OH- and dissolved oxygen in the solution to produce some active substances with strong redox ability, thereby promoting catalytic reactions or prompting exogenous catalysts to take effect. As a method of converting tiny mechanical energy around into chemical energy, tribocatalysis is almost unrestricted by external conditions and has been proven to be an effective means of utilizing mechanical energy. In 1999, Domen et al. found that water can be split into H by copper oxide, nickel monoxide, cobalt tetroxide and ferric tetroxide. 2 and O2 This is the first application of magnetic stirring in mechanical catalysis. In recent years, Chen Wanping et al. have reported TiO 2 Nanoparticles were magnetically stirred for 24 hours to generate 3.27 ppm of CO and the metal coating at the bottom of the reactor was changed to increase CO 2 The reducing properties make Co 3 O 4 The nanoparticles generated 10.08 ppm by magnetic stirring for 5 h. These studies all show that friction catalysis in CO 2 has great potential in reducing CO 2 The ability needs to be improved. Summary of the invention

[0005] In order to solve the above problems in the prior art, the present invention provides a method for reducing CO 2 A friction catalyst and its preparation method and application, the catalyst uses tungsten bronze material and zinc oxide to form a heterogeneous structure, which helps to expand the structural types of friction catalytic materials and reduce the harm of lead-based ceramics to human body and environment.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for reducing CO 2 The friction catalyst is a heterogeneous structure, and the chemical expression is Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O 6 @ZnO (BSNT@ZnO).

[0008] As a preferred embodiment of the present invention, the content of ZnO in the catalyst is 2.5-10 wt%.

[0009] The present invention also provides a method for reducing CO 2 The method for preparing a friction catalyst comprises the following steps:

[0010] (1) BaCO 3 、SrCO 3 , Nb 2 O 5 、 2 O 5 The mixture was ball-milled and dried in sequence to obtain sample Ⅰ;

[0011] (2) pressing and molding the sample I, and pre-calcining to obtain the sample II;

[0012] (3) Grinding the sample II, then ball milling, drying, pressing, cold isostatic pressing, sintering, and cooling to room temperature to obtain Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O 6 (BSNT);

[0013] (4) Weighing the BSNT prepared in step (3) and adding it to the anhydrous ethanol solution of ZnO, and sequentially performing ultrasonic treatment and stirring treatment to obtain sample III;

[0014] (5) Filter the sample III to collect the sediment, then wash, dry, sinter, and cool to room temperature to obtain the product for reducing CO 2 friction catalyst.

[0015] As a preferred embodiment of the present invention, in step (1), the molar ratio of Ba, Sr, Nb, Ta and O in the mixture is 0.75:0.25:1.9:0.1:6.

[0016] As a preferred embodiment of the present invention, in step (1) and step (3), the ball milling uses anhydrous ethanol as the ball milling medium, the ball milling speed is 250-350 r / min, and the time is 5-7 h.

[0017] As a preferred embodiment of the present invention, in step (1), step (3) and step (5), the drying temperature is 100-150° C. and the drying time is 3-5 hours.

[0018] Optionally, in step (1), step (3) and step (5), the drying temperature is independently selected from any value of 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or a range between any two of the above points.

[0019] Optionally, in step (1), step (3) and step (5), the drying time is independently selected from any value among 3h, 3.5h, 4h, 4.5h, 5h or a range value between any two of the above points.

[0020] As a preferred embodiment of the present invention, in step (2), the sample I is pressed and formed at 10-50 MPa; the pre-sintering temperature is 800-1200° C., and the time is 3-5 hours.

[0021] Optionally, in step (2), the pre-firing temperature is independently selected from any value among 800°C, 900°C, 1000°C, 1100°C, 1200°C or a range between any two of the above points.

[0022] Optionally, in step (2), the pre-burning time is independently selected from any value among 3h, 3.5h, 4h, 4.5h, 5h or a range between any two of the above points.

[0023] As a preferred embodiment of the present invention, in step (3), the cold isostatic pressing pressure is 150-250 MPa; in step (3), the sintering temperature is 1310-1350°C, the time is 5-10 h, and the heating rate during the sintering process is 4-6°C / min.

[0024] Optionally, in step (3), the cold isostatic pressing pressure is independently selected from any value among 150 MPa, 180 MPa, 200 MPa, 220 MPa, 250 MPa or a range of values ​​between any two of the above points.

[0025] Optionally, in step (3), the sintering temperature is independently selected from any value among 1310°C, 1320°C, 1330°C, 1340°C, 1350°C or a range between any two of the above points.

[0026] Optionally, in step (3), the sintering time is independently selected from any value among 5h, 6h, 7h, 8h, 9h, 10h or a range between any two of the above points.

[0027] Optionally, in step (3), the heating rate during the sintering process is independently selected from any value of 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, or a range between any two of the above points.

[0028] As a preferred embodiment of the present invention, in step (4), the mass of ZnO is 2.5-10wt% of the total mass of BSNT and ZnO; the time of ultrasound and stirring is 30-60min, the sintering temperature is 300-500°C, the time is 2-5h, and the heating rate during the sintering process is 4-6°C / min; in step (5), the sintering temperature is 400-600°C, and the time is 1-3h.

[0029] Optionally, in step (4), the content of the added ZnO is independently selected from any value of 2.5wt%, 5wt%, 7.5wt%, 10wt% by mass or a range between any two of the above points.

[0030] Optionally, in step (4), the ultrasound and stirring time are independently selected from any value among 30 min, 40 min, 50 min, 60 min or a range between any two of the above points.

[0031] Optionally, in step (4), the sintering time is independently selected from any value of 2h, 3h, 4h, 5h, or a range between any two of the above points.

[0032] The present invention also provides a method for reducing CO 2 The tribocatalysts in the reduction of CO 2 Application in.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention adopts a solid phase method to prepare a friction catalyst submicron powder material, which has a simple process and is harmless to the environment. 2 It has extremely strong reducing ability and can generate 274ppm of CO after 12 hours of friction catalysis.

[0035] (2) The reduction of CO provided by the present invention 2 The friction catalyst has good temperature stability and simple preparation method. It uses tungsten bronze material and zinc oxide to form a heterogeneous structure, which helps to expand the structural types of friction catalytic materials and reduce the harm of lead-based ceramics to the human body and the environment. 2 The generated CO can be used as feed gas for the Fischer-Tropsch synthesis reaction to produce high-carbon chemicals, which has good industrialization and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 This is an X-ray diffraction pattern of the BSNT@ZnO heterostructure catalyst prepared in Example 3 of the present invention;

[0038] Figure 2 This is a surface microscopic morphology photograph of the BSNT@ZnO heterogeneous structure catalyst prepared in Example 3 of the present invention;

[0039] Figure 3 This is a particle size distribution diagram of the BSNT@ZnO heterogeneous structure catalyst prepared in Example 3 of the present invention;

[0040] Figure 4 Tribocatalytic reduction of CO over BSNT@ZnO 2 Schematic diagram of the principle;

[0041] Figure 5The CO of the BSNT@ZnO heterogeneous structure catalyst prepared in Example 3 of the present invention 2 Restore data graph;

[0042] Figure 6 This is a diagram showing the friction catalytic cycle effect of the BSNT@ZnO heterostructure catalyst prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0043] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0044] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0047] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0048] Example 1

[0049] The preparation of the tribocatalyst for reducing CO2 is as follows:

[0050] (1) BaCO with a purity of 99.99% 3 、SrCO 3 , Nb 2 O5 、 2 O 5 Raw materials according to chemical formula Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O 6 The chemical stoichiometric ratio shown is put into the ball mill as BSNT raw material, and zirconium dioxide balls and nylon jars are selected; the total mass of the added raw materials is 8% of the mass of the grinding balls; the mixing ball milling time is 24 hours, the rotation speed is 180 rpm, and the ball milling medium is anhydrous ethanol.

[0051] (2) The product obtained in step (1) is placed in an oven at 120° C. and dried for 4 hours, pressed at 25 MPa, and then pre-sintered at 1000° C. at a heating rate of 5° C. / min for 4 hours; the pre-sintered powder is taken out and ground, and then ball-milled with anhydrous ethanol as a ball-milling medium for 24 hours to mix evenly, dried at 120° C. for 4 hours, ground into powder, and then pressed into discs, and cold isostatically pressed at a pressure of 200 MPa.

[0052] (3) The product obtained in step (2) was sintered at 1250°C in an air atmosphere in a high-temperature furnace and kept warm for 6 hours. The sample heating rate was 5°C / min. Finally, the sample was cooled to room temperature in the furnace. The obtained sample was crushed and placed in a high-energy ball mill at a speed of 300 rpm. Anhydrous ethanol was used as the ball milling medium for 24 hours. After drying in an oven at 120°C for 4 hours, it was ground into powder to obtain BSNT powder material.

[0053] (4) Weigh 0.2 g of the BSNT prepared in step (3), add 20 ml of anhydrous ethanol containing 0.0051 g of ZnO, ultrasonicate for 30 minutes, add three polytetrafluoroethylene (PTFE) rotors and stir for 30 minutes, filter and collect the sediment. Wash the sediment with deionized water and anhydrous ethanol, and put it into a 120°C drying oven for drying. After taking it out, put the sample into a muffle furnace at 500°C and calcine it at a speed of 5°C / min for 2 hours to obtain a BSNT@ZnO heterostructure catalyst with a ZnO mass fraction of 2.5wt%.

[0054] Example 2

[0055] The preparation of the tribocatalyst for reducing CO2 is as follows:

[0056] (1) BaCO with a purity of 99.99% 3 、SrCO 3 , Nb 2 O 5 、 2 O 5 Raw materials according to chemical formula Ba 0.75 Sr0.25 Nb 1.9 Ta 0.1 O 6 The chemical stoichiometric ratio shown is put into the ball mill as BSNT raw material, and zirconium dioxide balls and nylon jars are selected; the total mass of the added raw materials is 8% of the mass of the grinding balls; the mixing ball milling time is 24 hours, the rotation speed is 180 rpm, and the ball milling medium is anhydrous ethanol.

[0057] (2) The product obtained in step (1) is placed in an oven at 120° C. and dried for 4 hours, pressed at 10 MPa, and then pre-sintered at 1000° C. at a heating rate of 5° C. / min for 4 hours; the pre-sintered powder is taken out and ground, and then ball-milled with anhydrous ethanol as a ball-milling medium for 24 hours to mix evenly, dried at 120° C. for 4 hours, ground into powder, and then pressed into discs, and cold isostatically pressed at a pressure of 200 MPa.

[0058] (3) The product obtained in step (2) was sintered at 1300°C in an air atmosphere in a high-temperature furnace and kept warm for 6 hours. The sample heating rate was 5°C / min. Finally, the sample was cooled to room temperature in the furnace. The obtained sample was crushed and placed in a high-energy ball mill at a speed of 300 rpm. Anhydrous ethanol was used as the ball milling medium for 24 hours. After drying in an oven at 120°C for 4 hours, it was ground into powder to obtain BSNT powder material.

[0059] (4) Weigh 0.2 g of the BSNT prepared in step (3), add 20 ml of anhydrous ethanol containing 0.0162 g of zinc oxide, ultrasonicate for 30 minutes, add three PTFE rotors and stir for 30 minutes, filter and collect the sediment. Wash the sediment with deionized water and anhydrous ethanol, and dry it in a 120°C drying oven. After taking it out, put the sample into a muffle furnace at 500°C and calcine it at a speed of 5°C / min for 2 hours to obtain a BSNT@ZnO heterostructure catalyst with a ZnO mass fraction of 7.5wt%.

[0060] Example 3

[0061] The preparation of the tribocatalyst for reducing CO2 is as follows:

[0062] (1) BaCO with a purity of 99.99% 3 、SrCO 3 , Nb 2 O 5 、 2 O 5 Raw materials according to chemical formula Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O 6The chemical stoichiometric ratio shown is put into the ball mill as BSNT raw material, and zirconium dioxide balls and nylon jars are selected; the total mass of the added raw materials is 8% of the mass of the grinding balls; the mixing ball milling time is 24 hours, the rotation speed is 180 rpm, and the ball milling medium is anhydrous ethanol.

[0063] (2) The product obtained in step (1) is placed in an oven at 120° C. and dried for 4 hours, pressed at 50 MPa, and then pre-sintered at 1000° C. at a heating rate of 5° C. / min for 4 hours; the pre-sintered powder is taken out and ground, and then ball-milled with anhydrous ethanol as a ball milling medium for 24 hours to mix evenly, dried at 120° C. for 4 hours, ground into powder, and then pressed into discs, and cold isostatically pressed at a pressure of 200 MPa.

[0064] (3) The product obtained in step (2) was sintered at 1350°C in an air atmosphere in a high-temperature furnace and kept warm for 6 hours. The sample heating rate was 5°C / min. Finally, the sample was cooled to room temperature with the furnace. The obtained sample was crushed and placed in a high-energy ball mill at a speed of 300 rpm. Anhydrous ethanol was used as the ball milling medium for 24 hours. After drying in an oven at 120°C for 4 hours, it was ground into powder to obtain BSNT powder material.

[0065] (4) Weigh 0.2 g of the prepared BSNT, add 20 ml of anhydrous ethanol containing 0.0105 g of ZnO, ultrasonicate for 30 minutes, add three PTFE rotors and stir for 30 minutes, filter and collect the sediment. Use deionized water and anhydrous ethanol to wash the sediment, and then put it into a 120°C drying oven for drying. After taking it out, put the sample into a muffle furnace at 500°C and calcine it at a speed of 5°C / min for 2 hours to obtain a BSNT@ZnO heterostructure catalyst with a ZnO mass fraction of 5wt%.

[0066] Characterization of the BSNT@ZnO heterogeneous structure catalyst prepared in Example 3:

[0067] The BSNT@ZnO heterogeneous structure catalyst prepared in Example 3 was subjected to XRD powder diffraction analysis. Figure 1As shown, it can be seen that BSNT is a tungsten bronze phase (PDF card PDF#01-173-0126), and no impurities appear. The diffraction peaks at positions 31.750, 34.439, 36.251, 47.541, 56.553, and 62.868 in the XRD of the prepared BSNT@ZnO particles correspond to the crystal plane indices of ZnO nanoparticles (100), (002), (101), (102), (110), and (103), respectively, and indicate that the loaded ZnO is a pure cubic phase (PDF card number: PDF#01-079-2205), and no other impurities appear. The XRD results show that the present invention successfully synthesized the BSNT@ZnO heterojunction.

[0068] Figure 2 , 3 The surface microscopic morphology and particle size distribution of BSNT@ZnO prepared in Example 3 show that the particle size of BSNT@ZnO powder is between 60 and 400 nm, and the average particle size is 180 nm, indicating that the size of BSNT@ZnO catalyst powder is submicron.

[0069] The characterization results of the BSNT@ZnO heterogeneous structure catalyst prepared in Examples 1-2 are consistent with those in Example 3.

[0070] Tribocatalytic reduction of CO 2 The effect verification:

[0071] 100 mg of BSNT@ZnO powder prepared in Example 3, 50 mL of deionized water, and three magnetic stirring bars were added into a quartz reactor (100 mL) in sequence. 2 After the gas is bubbled, the reactor is sealed. A magnetic stirrer is used to drive the PTFE magnet to stir the water in the reactor at a speed of 300 r / min, and the reactor is placed in a dark environment. After the reaction is completed, a meteorological mass spectrometer is used to collect the gas in the reactor to test the content of the generated gas. Figure 4 Tribocatalytic reduction of CO over BSNT@ZnO 2 Schematic diagram of the principle. Figure 5 This is the final test result, indicating that 274 ppm of CO can be generated after 12 hours of friction catalysis. Figure 6 It is the gas production after one, two, three and four cycles. It was further found that after five cycles, 265 ppm of CO was generated, which was 6 ppm lower than that after four cycles, but the gas production was still high. The data showed that the prepared friction catalyst had good stability.

[0072] Comparative Example 1

[0073] The same as Example 3, except that the amount of raw materials in step (1) is adjusted as follows:

[0074] (1) BaCO with a purity of 99.99% 3 、SrCO 3 , Nb 2 O 5 、 2 O 5 The raw materials are put into a ball mill as BSNT raw materials in a molar ratio of 0.5:0.5:1.4:0.6:6, and zirconium dioxide balls and nylon cans are selected; the total mass of the added raw materials is 8% of the mass of the grinding balls; the mixed ball milling time is 24 hours, the rotation speed is 180 rpm, and the ball milling medium is anhydrous ethanol.

[0075] The other steps are the same as those in Example 3.

[0076] Comparative Example 2

[0077] The same as Example 3, except that in step (2), the pre-sintering operation is omitted, and the details are as follows:

[0078] (2) The product obtained in step (1) is placed in an oven at 120° C. and dried for 4 hours, pressed into a shape at 50 MPa, ground, and then ball-milled with anhydrous ethanol as a ball-milling medium for 24 hours to mix evenly, dried at 120° C. for 4 hours, ground into powder, and then pressed into discs, and cold isostatically pressed at a pressure of 200 MPa.

[0079] The other steps are the same as those in Example 3.

[0080] Comparative Example 3

[0081] The same as Example 3, except that in step (2), the cold isostatic pressing operation is omitted, and the details are as follows:

[0082] (2) The product obtained in step (1) is placed in an oven at 120° C. and dried for 4 hours, pressed at 50 MPa, and then pre-sintered at 1000° C. at a heating rate of 5° C. / min for 4 hours; the pre-sintered powder is taken out and ground, and then ball-milled with anhydrous ethanol as a ball-milling medium for 24 hours to mix evenly, dried at 120° C. for 4 hours, ground into powder, and then pressed into discs.

[0083] The other steps are the same as those in Example 3.

[0084] The final products prepared in Comparative Examples 1 to 3 were found to be non-heterogeneous structures. The same method as above was used to test their CO 2The results showed that after 12 hours of friction catalysis, 187, 156, and 148 ppm of CO could be generated respectively. After four cycles, 173, 146, and 135 ppm of CO could be generated respectively.

[0085] The BSNT powder material prepared in step (3) of Example 3 was tested for its CO 2 The results showed that after 12 hours of friction catalysis, 185 ppm of CO could be generated, and after four cycles, 170 ppm of CO could be generated.

[0086] The present invention uses a certain amount of ferroelectric material and ZnO to construct a heterojunction for friction catalytic reduction of CO 2 , greatly improving the CO 2 The research found that when the type and amount of raw materials are changed, or when the pre-sintering and cold isostatic pressing operations are omitted during the preparation process, the structure of the resulting product will also change, which will have a significant impact on the reduction of CO. 2 The reduction capacity of CO will deteriorate. The study also found that BSNT alone can reduce CO 2 , but the efficiency is lower because no heterojunction is formed.

[0087] The above description is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, and they should be covered by the protection scope of the present invention.

Claims

1. A friction catalyst for reducing CO2, characterized in that: The catalyst is a heterogeneous structure, and the chemical expression is Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O6@ZnO.

2. The friction catalyst for reducing CO2 according to claim 1, characterized in that: The content of ZnO in the catalyst is 2.5-10 wt%.

3. A method for preparing a friction catalyst for reducing CO2 according to claim 1 or 2, characterized in that: The following steps are involved: (1) A mixture containing BaCO3, SrCO3, Nb2O5, and Ta2O5 is ball-milled and dried in sequence to obtain sample I; (2) pressing and molding the sample I, and pre-calcining to obtain the sample II; (3) Grinding the sample II, and then sequentially subjecting it to ball milling, drying, pressing, cold isostatic pressing, and sintering to obtain Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O6; (4) Weigh the Ba prepared in step (3) 0.75 Sr 0.25 Nb 1.9 Ta 0.1 O6 was added to the anhydrous ethanol solution of ZnO, and then subjected to ultrasonic and stirring treatments to obtain sample III; (5) Filter the sample III to collect the sediment, and then wash, dry and sinter it in sequence to obtain the friction catalyst for reducing CO2.

4. The preparation method according to claim 3, characterized in that: In step (1), the molar ratio of Ba, Sr, Nb, Ta and O in the mixture is 0.75:0.25:1.9:0.1:

6.

5. The preparation method according to claim 3, characterized in that: In step (1) and step (3), the ball milling uses anhydrous ethanol as the ball milling medium, the ball milling speed is 250-350 r / min, and the time is 5-7 h.

6. The preparation method according to claim 3, characterized in that: In step (1), step (3) and step (5), the drying temperature is 100-150° C. and the drying time is 3-5 hours.

7. The preparation method according to claim 3, characterized in that: In step (2), the pre-firing temperature is 800-1200° C. and the time is 3-5 hours.

8. The preparation method according to claim 3, characterized in that: In step (3), the cold isostatic pressing pressure is 150-250 MPa; in step (3), the sintering temperature is 1310-1350°C, the time is 5-10 hours, and the heating rate during the sintering process is 4-6°C / min.

9. The preparation method according to claim 3, characterized in that: In step (4), the mass of ZnO is Ba 0.75 Sr 0.25 Nb 1.9 Ta 0.1 The total mass of O6 and ZnO is 2.5-10wt%; the ultrasonic and stirring time are both 30-60min; in step (5), the sintering temperature is 400-600°C and the time is 1-3h.

10. Use of the friction catalyst for reducing CO2 according to claim 1 or 2 in reducing CO2.