Grease for new energy vehicle motor bearings for reducing shaft current and preparation method thereof
By using conductive additive-enhanced grease in the bearings of new energy vehicle motors, the electrocorrosion problem caused by the shaft current at the 800V platform is solved, and the high and low temperature performance and conductive properties of the bearing are achieved, extending the service life.
Patent Information
- Application Number
- CN202410130312.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-01-31
AI Technical Summary
The shaft current generated by the new energy vehicle drive motor under the 800V platform causes the bearing to be electrocorrosive, overheated and burned. The existing methods to prevent electrocorrosion are difficult to apply to miniaturized new energy vehicle drive motors, and the grease needs to have high and low temperature performance.
Use synthetic base oil, dodecyl stearic acid, sebacic acid, lithium hydroxide, antioxidants, anti-wear pressure agents and conductive additives (such as conductive carbon black, conductive graphite, nanocarbon fiber, carbon nanotubes, graphene ) The grease composed of ) improves the conductivity performance through conductive additives and reduces the accumulation of shaft current.
The grease has low volume resistivity, excellent high and low temperature performance, which reduces the generation of shaft current and extends the service life of the bearing.
Smart Images

Figure BDA0004689588690000091 
Figure BDA0004689588690000101 
Figure BDA0004689588690000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of grease preparation, and in particular to a grease for a new energy vehicle motor bearing that reduces shaft current and a preparation method thereof. Background Art
[0002] With the upgrading of new energy vehicles in recent years, the drive motors at home and abroad are developing towards high voltage. 800V voltage is considered to be the only way for the next generation of new energy electric vehicles and has become the commanding height of the new round of competition among automakers. 800V voltage can significantly reduce the diameter of high-voltage wire harnesses, reduce heat generation, reduce cable diameter and weight, and save the cost and installation space of wire harnesses.
[0003] However, the probability of the drive motor generating shaft current under the 800V platform increases significantly. The shaft current passes through the circuit formed by the rotating shaft, bearing and base plate, causing electro-corrosion pitting or washboard-like burn marks on the journal and bearing or causing the rolling bearing to overheat and burn, thereby significantly affecting the service life of the bearing.
[0004] In order to reduce the damage to bearings caused by shaft current, the following two methods are generally used: one is to add an insulating pad at the non-load end to block the shaft current; the other is to use carbon brushes to short-circuit the bearings at both ends of the motor to prevent the shaft current from passing through the bearings.
[0005] However, the above two methods of preventing electrocorrosion can generally only be used for large motors, which is very difficult to implement for the increasingly miniaturized new energy vehicle drive motors. In addition, new energy vehicle drive motor bearings generally use grease as a lubricant, which requires the grease to have good high and low temperature performance. Summary of the invention
[0006] The purpose of the present application is to provide a grease for new energy vehicle motor bearings that reduces shaft current and a preparation method thereof. The grease has excellent high and low temperature performance and friction and anti-wear capabilities, and excellent conductive function, making it difficult for shaft voltage to accumulate, thereby reducing the generation of shaft current.
[0007] The above-mentioned invention objective of the present application is achieved through the following technical solutions:
[0008] A lubricating grease for a new energy vehicle motor bearing for reducing shaft current is prepared from raw materials including the following components, calculated by mass percentage:
[0009] Synthetic base oil 65%~84.8%;
[0010] Dodecyl hydroxystearic acid 8% to 15%;
[0011] Sebacic acid 2%-5%;
[0012] Lithium hydroxide 2% to 5%;
[0013] Antioxidants 0.2% to 3%;
[0014] Anti-wear extreme pressure agent 1% to 5%;
[0015] Conductive additives 2% to 5%;
[0016] Wherein, the conductive additive is one or more of conductive carbon black Super P, Ketjen black, conductive graphite KS-6, nanocarbon fiber VGCF, carbon nanotubes, and graphene;
[0017] The sum of the mass percentages of the above components is 100%.
[0018] By adding conductive additives, the conductivity of grease is improved, thereby reducing the accumulation of shaft current; among them, conductive carbon black Super P has a high specific surface area and good conductivity, providing excellent charge transfer capability and capacitor energy storage performance; Ketjen black is a carbon black produced by a special production process and has extremely high conductivity; conductive graphite KS-6 can complement conductive carbon black to improve conductivity; nano-carbon fiber VGCF is evenly distributed in the grease as a conductive agent to form a uniform point-line connected conductive network; carbon nanotubes and graphene both have high conductivity, mechanical properties and chemical stability.
[0019] In a preferred example, the present application can be further configured as follows: the conductive additives are conductive carbon black Super P and conductive graphite KS-6, and the weight ratio of conductive carbon black Super P to conductive graphite KS-6 is 1:1.
[0020] Conductive graphite KS-6 is combined with conductive carbon black Super P to make up for the shortcomings of conductive carbon black Super P: conductive carbon black has a large specific surface area and conductivity, which is an important factor in its conductive performance, and the size of conductive graphite in the single crystal range is several times larger than that in carbon black particles. Conductive carbon black can be better filled into the material or composition during the filling process to improve its conductive performance. Due to its large particle size, conductive graphite can provide a better conductive network and improve the overall conductive performance of the material, thereby producing complementary properties. The weight ratio of conductive graphite KS-6 and conductive carbon black Super P is set to 1:1 to improve their complementary effect, thereby greatly improving the conductive performance of the grease.
[0021] In a preferred example, the present application can be further configured as follows: the synthetic base oil is a poly-alpha-olefin synthetic base oil.
[0022] Polyalphaolefin synthetic base oil is a base oil made by polymerization of ethylene to form alpha olefin, and then further polymerization and hydrogenation. It has good viscosity-temperature performance and low-temperature fluidity. According to the viscosity, it can be divided into low-viscosity PAO, medium-viscosity PAO and high-viscosity PAO; among them, low-viscosity PAO includes: PAO2, PAO2.5, PAO4, PAO5, PAO6, PAO7, PAO8, PAO9, PAO10, etc.; medium-viscosity PAO includes: PAO25, etc.; high-viscosity PAO includes: PAO40, PAO100, PAO150, PAO300, etc.
[0023] In a preferred example, the present application can be further configured as follows: the antioxidant is an amine antioxidant, specifically one of diphenylamine or diisooctyldiphenylamine.
[0024] Amines, especially one of diphenylamine or diisooctyldiphenylamine, are used as antioxidants, which have excellent antioxidant properties, thermal stability and rust resistance. Their excellent antioxidant properties can effectively inhibit the oxidation reaction of grease under high temperature, high pressure, oxidation and other conditions, thereby extending the service life of the grease; their good thermal stability can effectively reduce the viscosity drop rate of the grease at high temperatures, thereby maintaining the lubricating properties of the grease; their good rust resistance can effectively inhibit rust on the metal surface, thereby protecting the metal from corrosion and extending the service life of the metal.
[0025] In a preferred example, the present application can be further configured as follows: the anti-wear extreme pressure agent is an organic sulfide, specifically one or more of dialkyl zinc dithiophosphate and triphenyl thiophosphate.
[0026] Organic sulfides, especially one or more of dialkyl zinc dithiophosphate and triphenyl thiophosphate, are used as anti-wear extreme pressure agents. They have excellent anti-wear extreme pressure properties, thermal stability and corrosion resistance. Organic sulfides are usually used together with other additives such as antioxidants and rust inhibitors to produce a synergistic effect to further improve the performance of grease.
[0027] The present application also provides a method for preparing a lubricating grease for a new energy vehicle motor bearing for reducing shaft current according to the present invention, comprising the following steps:
[0028] 1) adding part of the synthetic base oil into a reaction kettle according to the proportion, and heating the reaction kettle to 60° C. to 70° C.;
[0029] 2) adding the dodecyl hydroxystearic acid and the sebacic acid into a reaction kettle according to the ratio, mixing and stirring evenly;
[0030] 3) dissolving the lithium hydroxide in water, adding 1 / 2 of the aqueous solution of lithium hydroxide into a reactor according to a ratio and stirring for 60 min to 90 min, and dropping the remaining aqueous solution of lithium hydroxide into the reactor during the stirring process;
[0031] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0032] 5) adding the remaining synthetic base oil into the reactor according to the proportion and heating to 210° C. to 215° C., keeping the temperature for 5 min to 10 min, and stopping heating after the holding time;
[0033] 6) After cooling to below 90° C., add the antioxidant, the anti-wear extreme pressure agent and the conductive additive in order according to the proportion, and stir for 20 min to 30 min;
[0034] 7) After grinding three times with a three-roll mill, the product is obtained.
[0035] In the above steps, the base oil is added in multiple times. Firstly, during the process of mixing and heating the base oil with dodecyl stearic acid and sebacic acid, the reaction system is easy to expand and overflow out of the reaction container; secondly, if all the base oil is added at one time, the concentration of the remaining substances in the reaction system is low, and the raw materials are not easy to contact each other, resulting in incomplete saponification reaction, which in turn affects the performance of the grease.
[0036] In summary, this application has the following beneficial technical effects:
[0037] 1. The grease prepared in the present application has a low volume resistivity and good electrical conductivity, thereby being able to reduce the shaft current generated by the motor during use;
[0038] 2. The grease prepared in this application has good high temperature performance, with a dropping point above 280°C, and still has good lubrication effect at high temperatures;
[0039] 3. The lubricating grease prepared in the present application has a low viscosity at -40°C and has good low-temperature performance. DETAILED DESCRIPTION
[0040] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0041] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components and / or combinations thereof. It should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention.
[0042] As mentioned above, the probability of driving the motor to generate shaft current under the 800V platform has increased significantly. The shaft current passes through the circuit formed by the rotating shaft, bearing and base plate, and produces electro-corrosion pitting or washboard-like burn marks on the journal and bearing or causes the rolling bearing to overheat and burn, thereby significantly affecting the service life of the bearing. Therefore, there is an urgent need to provide a grease for new energy vehicle motor bearings that can reduce shaft current and a preparation method thereof.
[0043] The present invention provides a grease for a new energy vehicle motor bearing for reducing shaft current and a preparation method thereof. The grease prepared by the method not only has excellent high and low temperature performance, but also has excellent electrical conductivity, making it difficult for shaft voltage to accumulate, thereby reducing the generation of shaft current.
[0044] The present application discloses a lubricating grease for a new energy vehicle motor bearing for reducing shaft current, which is prepared from raw materials including the following components by mass percentage:
[0045] Synthetic base oil 65%~84.8%;
[0046] Dodecyl hydroxystearic acid 8% to 15%;
[0047] Sebacic acid 2%-5%;
[0048] Lithium hydroxide 2% to 5%;
[0049] Antioxidants 0.2% to 3%;
[0050] Anti-wear extreme pressure agent 1% to 5%;
[0051] Conductive additives 2% to 5%;
[0052] Wherein, the conductive additive is one or more of conductive carbon black Super P, Ketjen black, conductive graphite KS-6, nanocarbon fiber VGCF, carbon nanotubes, and graphene;
[0053] The sum of the mass percentages of the above components is 100%.
[0054] Preferably, the conductive additives are conductive carbon black Super P and conductive graphite KS-6, and the weight ratio of conductive carbon black Super P to conductive graphite KS-6 is 1:1. Conductive carbon black can be better filled into the material or composition during the filling process to improve its conductive properties, and conductive graphite can provide a better conductive network due to its large particle size, thereby improving the overall conductive properties of the material, thereby producing complementary properties. The weight ratio of conductive graphite KS-6 to conductive carbon black Super P is set to 1:1 to improve their complementary effect, thereby greatly improving the conductive properties of the grease.
[0055] Preferably, the synthetic base oil is a poly-α-olefin synthetic base oil, which has good viscosity-temperature properties and low-temperature fluidity, and can effectively reduce the friction coefficient of the friction surface and improve the anti-wear performance of the grease.
[0056] Preferably, the antioxidant is an amine antioxidant, specifically one of diphenylamine or diisooctyldiphenylamine. Diphenylamine and diisooctyldiphenylamine have good stability at high temperatures and good antioxidant properties, and can effectively prevent or delay the oxidative degradation of polymer materials, thereby significantly improving the stability of the materials.
[0057] Preferably, the anti-wear extreme pressure agent is an organic sulfide, specifically one or more of dialkyl zinc dithiophosphate and triphenyl thiophosphate. The organic sulfide has excellent anti-wear extreme pressure properties and synergizes with antioxidants to improve the antioxidant properties of grease.
[0058] The above-mentioned grease for reducing shaft current of a new energy vehicle motor bearing comprises the following steps:
[0059] 1) adding part of the synthetic base oil into a reaction kettle according to the proportion, and heating the reaction kettle to 60° C. to 70° C.;
[0060] 2) adding the dodecyl hydroxystearic acid and the sebacic acid into a reaction kettle according to the ratio, mixing and stirring evenly;
[0061] 3) dissolving the lithium hydroxide in water, adding 1 / 2 of the aqueous solution of lithium hydroxide into a reactor according to a ratio and stirring for 60 min to 90 min, and dropping the remaining aqueous solution of lithium hydroxide into the reactor during the stirring process;
[0062] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0063] 5) adding the remaining synthetic base oil into the reactor according to the proportion and heating to 210° C. to 215° C., keeping the temperature for 5 min to 10 min, and stopping heating after the holding time;
[0064] 6) After cooling to below 90° C., add the antioxidant, the anti-wear extreme pressure agent and the conductive additive in order according to the proportion, and stir for 20 min to 30 min;
[0065] 7) After grinding three times with a three-roll mill, the product is obtained.
[0066] The present invention is further explained by the following examples, but it is not intended to limit the present invention. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0067] Example 1
[0068] A grease for a new energy vehicle motor bearing that reduces shaft current uses conductive carbon black Super P as a conductive additive. The raw material ratio for its preparation is shown in Table 1.
[0069] Table 1
[0070] Raw material name Proportion,% PAO10 79% Dodecyl Hydroxystearic Acid 9% Sebacic acid 3% Lithium hydroxide 2.8% Diisooctyl diphenylamine 0.2% Zinc dialkyl dithiophosphate 2% Triphenyl phosphorothioate 2% Conductive carbon black SuperP 2%
[0071] The method for preparing the above-mentioned grease for reducing shaft current for new energy vehicle motor bearings comprises the following steps:
[0072] 1) Add 500g of PAO10 into the reactor and heat it to 60℃~70℃;
[0073] 2) adding 90 g of dodecyl hydroxystearic acid and 30 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0074] 3) dissolving 14 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution into a reactor and stirring for 60 min, dissolving the remaining 14 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise into the reactor during stirring;
[0075] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0076] 5) Add 290 g of PAO10 into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0077] 6) After cooling to below 90° C., add 2 g of diisooctyl diphenylamine, 20 g of zinc dialkyl dithiophosphate, 20 g of triphenyl thiophosphate and 20 g of conductive carbon black Super P in sequence and stir for 30 min;
[0078] 7) After grinding three times with a three-roll mill, the product is obtained.
[0079] Example 2
[0080] A grease for a new energy vehicle motor bearing that reduces shaft current uses conductive carbon black Super P and carbon nanotubes as conductive additives. The raw material ratio for its preparation is shown in Table 2.
[0081] Table 2
[0082]
[0083]
[0084] The method for preparing the above-mentioned grease for reducing shaft current for new energy vehicle motor bearings comprises the following steps:
[0085] 1) Add 500g of PAO8 into the reactor and heat it to 60℃~70℃;
[0086] 2) adding 93 g of dodecyl hydroxystearic acid and 31 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0087] 3) dissolving 14.5 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution to a reactor and stirring for 90 min, dissolving the remaining 14.5 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise to the reactor during stirring;
[0088] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0089] 5) Add 300 g of PAO8 into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0090] 6) After cooling to below 90° C., 2 g of diphenylamine, 10 g of zinc dialkyl dithiophosphate, 15 g of triphenyl thiophosphate, 10 g of carbon nanotubes and 10 g of conductive carbon black Super P were added in sequence and stirred for 30 min;
[0091] 7) After grinding three times with a three-roll mill, the product is obtained.
[0092] Example 3
[0093] A grease for a new energy vehicle motor bearing for reducing shaft current, using conductive carbon black Super P and conductive graphite KS-6 as conductive additives, and the weight ratio of conductive carbon black Super P to conductive graphite KS-6 is 1:1. The raw material ratio for its preparation is shown in Table 3.
[0094] Table 3
[0095] Raw material name Proportion,% PAO8 80% Dodecyl Hydroxystearic Acid 9.3% Sebacic acid 3.1% Lithium hydroxide 2.9% Diphenylamine 0.2% Zinc dialkyl dithiophosphate 1% Triphenyl phosphorothioate 1.5% Conductive carbon black SuperP 1% Conductive graphite KS-6 1%
[0096] The method for preparing the above-mentioned grease for reducing shaft current for new energy vehicle motor bearings comprises the following steps:
[0097] 1) Add 450 g of PAO8 into the reactor and heat it to 60°C to 70°C;
[0098] 2) adding 93 g of dodecyl hydroxystearic acid and 31 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0099] 3) dissolving 14.5 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution to a reactor and stirring for 90 min, dissolving the remaining 14.5 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise to the reactor during stirring;
[0100] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0101] 5) Add 350 g of PAO10 into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0102] 6) After cooling to below 90° C., 2 g of diisooctyl diphenylamine, 10 g of zinc dialkyl dithiophosphate, 15 g of triphenyl thiophosphate, 10 g of conductive carbon black Super P and 10 g of conductive graphite KS-6 were added in sequence and stirred for 30 min;
[0103] 7) After grinding three times with a three-roll mill, the product is obtained.
[0104] Example 4
[0105] A grease for a new energy vehicle motor bearing that reduces shaft current uses conductive carbon black Super P and nano-carbon fiber VGCF as conductive additives. The raw material ratio for its preparation is shown in Table 4.
[0106] Table 4
[0107]
[0108]
[0109] The method for preparing the above-mentioned grease for reducing shaft current for new energy vehicle motor bearings comprises the following steps:
[0110] 1) Add 500g of PAO10 into the reactor and heat it to 60℃~70℃;
[0111] 2) adding 93 g of dodecyl hydroxystearic acid and 31 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0112] 3) dissolving 14.5 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution to a reactor and stirring for 90 min, dissolving the remaining 14.5 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise to the reactor during stirring;
[0113] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0114] 5) Add 300 g of PAO8 into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0115] 6) After cooling to below 90°C, 2 g of diisooctyl diphenylamine, 15 g of dialkyl zinc dithiophosphate, 10 g of triphenyl thiophosphate, 10 g of conductive carbon black Super P and 10 g of nanocarbon fiber VGCF were added in sequence and stirred for 30 min;
[0116] 7) After grinding three times with a three-roll mill, the product is obtained.
[0117] Example 5
[0118] A grease for a new energy vehicle motor bearing that reduces shaft current uses conductive carbon black Super P and Ketjen black as conductive additives. The raw material ratio for its preparation is shown in Table 5.
[0119] Table 5
[0120]
[0121]
[0122] The method for preparing the above-mentioned grease for reducing shaft current for new energy vehicle motor bearings comprises the following steps:
[0123] 1) Add 400g of PAO10 into the reactor and heat it to 60℃~70℃;
[0124] 2) adding 93 g of dodecyl hydroxystearic acid and 31 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0125] 3) dissolving 14.5 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution to a reactor and stirring for 90 min, dissolving the remaining 14.5 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise to the reactor during stirring;
[0126] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0127] 5) Add 400 g of PAO8 into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0128] 6) After cooling to below 90°C, add 2 g of diisooctyl diphenylamine, 15 g of zinc dialkyl dithiophosphate, 10 g of triphenyl thiophosphate, 10 g of conductive carbon black Super P and 10 g of Ketjen black in sequence and stir for 30 min;
[0129] 7) After grinding three times with a three-roll mill, the product is obtained.
[0130] Example 6
[0131] A grease for new energy vehicle motor bearings that reduces shaft current uses carbon nanotubes and graphene as conductive additives. The raw material ratio for its preparation is shown in Table 6.
[0132] Table 6
[0133] Raw material name Proportion,% PAO10 35% PAO8 45% Dodecyl Hydroxystearic Acid 9.3% Sebacic acid 3.1% Lithium hydroxide 2.9% Diisooctyl diphenylamine 0.2% Zinc dialkyl dithiophosphate 1% Triphenyl phosphorothioate 1.5% Carbon Nanotubes 1% Graphene 1%
[0134] The method for preparing the above-mentioned grease for reducing shaft current for new energy vehicle motor bearings comprises the following steps:
[0135] 1) Add 500g of PAO8 into the reactor and heat it to 60℃~70℃;
[0136] 2) adding 93 g of dodecyl hydroxystearic acid and 31 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0137] 3) dissolving 14.5 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution to a reactor and stirring for 90 min, dissolving the remaining 14.5 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise to the reactor during stirring;
[0138] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0139] 5) Add 300 g of PAO8 into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0140] 6) After cooling to below 90° C., 2 g of diphenylamine, 10 g of zinc dialkyl dithiophosphate, 15 g of triphenyl thiophosphate, 10 g of carbon nanotubes and 10 g of graphene were added in sequence and stirred for 30 min;
[0141] 7) After grinding three times with a three-roll mill, the product is obtained.
[0142] Comparative Example 1
[0143] The grease prepared by using 500N as the base oil and without adding conductive additives is used as a comparative example. The raw material ratios for its preparation are shown in Table 7.
[0144] Table 7
[0145]
[0146]
[0147] The preparation method of the grease of Comparative Example 1 comprises the following steps:
[0148] 1) Add 500g of 500N into the reactor and heat it to 60℃~70℃;
[0149] 2) adding 90 g of dodecyl hydroxystearic acid and 30 g of sebacic acid into a reaction kettle and mixing and stirring evenly;
[0150] 3) dissolving 14 g of lithium hydroxide in 60 g of water, adding the lithium hydroxide aqueous solution to a reactor and stirring for 90 min, dissolving the remaining 14 g of lithium hydroxide in 60 g of water, and adding the remaining lithium hydroxide aqueous solution dropwise to the reactor during stirring;
[0151] 4) The mixture in the reactor was heated to 100°C to 110°C and dehydrated for 60 minutes;
[0152] 5) Add 310 g of 500N into the reactor and heat to 210°C for 10 min. After the heat preservation time, stop heating;
[0153] 6) After cooling to below 90°C, add 2 g of diphenylamine, 20 g of triphenyl thiophosphate and 20 g of zinc dialkyl dithiophosphate in sequence and stir for 30 min;
[0154] 7) After grinding three times with a three-roll mill, the product is obtained.
[0155] The performance test data of Examples 1-6 and Comparative Example 1 are shown in Table 8.
[0156] Table 8
[0157]
[0158]
[0159] In summary, it can be seen from Table 8 that the present invention provides a kind of grease for reducing shaft current for new energy vehicle motor bearings and its preparation method. Compared with Comparative Example 1, the similar viscosity of the grease Examples 1-6 prepared in this application under -40°C environment is relatively small, and its dropping point is above 280°C, indicating that it has good high and low temperature performance; at the same time, the volume resistivity of Examples 1-6 is lower than that of Comparative Example 1, indicating that it has good electrical conductivity, and Example 3 has the lowest volume resistivity and the best electrical conductivity, which is the optimal solution. The grease prepared in this application makes it difficult for the shaft voltage of the motor bearing of new energy vehicles to accumulate, thereby reducing the generation of shaft current, and has broad application prospects.
[0160] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A grease for new energy vehicle motor bearings that reduces shaft current. Features: The raw materials are prepared from the following components by weight percentage: Synthetic base oil 65%~84.8%; Dodecyl hydroxystearic acid 8%~15%; Sebacic acid 2%~5%; Lithium hydroxide 2%~5%; Antioxidants 0.2%~3%; Anti-wear extreme pressure agent 1%~5%; Conductive additives 2%~5%; Wherein, the sum of the mass percentages of the above components is 100%; Wherein, the conductive additive is conductive carbon black Super P and conductive graphite KS-6, and the weight ratio of conductive carbon black Super P to conductive graphite KS-6 is 1:1; The lubricating grease for the motor bearing of a new energy vehicle for reducing shaft current, and the preparation method thereof, comprise the following steps: Add part of the synthetic base oil into the reactor according to the ratio, and heat it to 60°C~70°C; Add the dodecyl hydroxystearic acid and the sebacic acid into the reaction kettle according to the ratio and mix and stir evenly; Dissolve the lithium hydroxide in water, add 1 / 2 of the aqueous solution of lithium hydroxide into the reactor according to the ratio and stir for 60 min to 90 min, and add the remaining aqueous solution of lithium hydroxide dropwise into the reactor during the stirring process; The mixture in the reactor was heated to 100°C~110°C and dehydrated for 60 minutes; Add the remaining synthetic base oil into the reactor according to the ratio and heat it to 210°C to 215°C, keep it warm for 5min to 10min, and stop heating after the warming time; After cooling to below 90° C., adding the antioxidant, the anti-wear extreme pressure agent and the conductive additive in order according to the proportion, and stirring for 20 min to 30 min; After grinding three times with a three-roll mill, the product is obtained.
2. A lubricating grease for a new energy vehicle motor bearing for reducing shaft current according to claim 1, Features: The synthetic base oil is a poly-alpha-olefin synthetic base oil.
3. A lubricating grease for a new energy vehicle motor bearing for reducing shaft current according to claim 1, Features: The antioxidant is an amine antioxidant, specifically one of diphenylamine or diisooctyldiphenylamine.
4. A lubricating grease for a new energy vehicle motor bearing for reducing shaft current according to claim 1, Features: The anti-wear extreme pressure agent is an organic sulfide, specifically one or more of dialkyl zinc dithiophosphate and triphenyl thiophosphate.