Ion sieve and its preparation method and application and preparation method of chemically strengthened glass

The ion sieve with a tailored SiO2, Al2O3, B2O3, and Na2O composition addresses lithium ion recycling inefficiencies, ensuring effective lithium recovery and preventing salt bath poisoning in chemically strengthened glass production.

CN118079856BActive Publication Date: 2024-12-03CHONGQING AUREAVIA HI TECH GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311769978.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-12-03
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Existing ion sieve materials used in chemically strengthened glass manufacturing are ineffective in efficiently recycling lithium ions, leading to salt bath 'poisoning' and adverse mechanical properties in the glass product.

Method used

An ion sieve with a specific composition of SiO2, Al2O3, B2O3, and Na2O, optimized to achieve high lithium ion absorption and easy acid hydrolysis, allowing for efficient recovery and reuse of lithium ions.

Benefits of technology

The ion sieve effectively absorbs lithium ions during glass manufacturing, preventing salt bath poisoning and enabling simple recovery of reusable lithium-containing materials, aligning with sustainable development goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004622660460000191
    Figure BDA0004622660460000191
  • Figure BDA0004622660460000192
    Figure BDA0004622660460000192
  • Figure BDA0004622660460000193
    Figure BDA0004622660460000193
Patent Text Reader

Abstract

The present application relates to an ion sieve and a preparation method and application thereof. The ion sieve comprises the following composition expressed in terms of molar percentage of oxides: SiO 2 20.00~50.00mol%Al 2 O 3 2.00~20.00mol%B 2 O 3 0.00~15.00mol% and Na 2 O 40.00~70.00mol%; wherein the composition of the ion sieve satisfies: 40.00mol%≤SiO 2 +Al 2 O 3 +B 2 O 3 ≤55.00mol%;0<(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <0.40;0.35<Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )‑(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <1.85. The ion sieve of the present application has a specific structure, and has the performance advantages of high lithium ion absorption rate and easy acid decomposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of ion sieves, and in particular to an ion sieve and a preparation method and application thereof, as well as a preparation method of chemically strengthened glass. Background Art

[0002] Chemically strengthened glass that has been chemically strengthened by ion exchange or the like is commonly used as protective glass for portable electronic devices and as glass substrates for displays. Common chemically strengthened glass refers to glass with better mechanical properties obtained by immersing the glass in a molten salt bath to exchange alkali metal ions with small ion radius in the glass with alkali metal ions with large ion radius in the molten salt bath, thereby forming a compressive stress layer on the glass surface.

[0003] Lithium-containing glass is a glass material that can obtain a deep compressive stress layer depth through ion exchange (for example, replacing Li ions with Na ions or K ions). Therefore, in recent years, the glass industry has introduced lithium aluminosilicate glass to prepare chemically strengthened glass.

[0004] In the chemical strengthening of lithium-containing glass, the lithium released from the glass into the molten salt bath accumulates as impurity ions, which hinders ion exchange and may cause undesirable stress distribution in the chemically strengthened glass product, such as lower compressive stress and / or shallower compression depth, which in turn adversely affects the mechanical properties of the glass product. This is so-called "poisoning" of the salt bath, and the accumulated lithium ions can be called "poisoning" ions.

[0005] In response to this, the inventors have developed an ion sieve material that can selectively absorb lithium ions, which is used as an absorption / adsorption material for impurity lithium ions in the salt bath, thereby controlling the lithium ion concentration in the salt bath, restoring the performance of the salt bath, and avoiding the "poisoning" phenomenon in the salt bath. The ion sieve material developed by the inventors mainly uses the free alkali metal cations in the ion sieve network architecture to exchange ions with impurity lithium ions in the salt bath, so that the lithium ions in the salt bath diffuse into the ion sieve channel and are selectively absorbed by the ion sieve. Summary of the invention

[0006] After further research on the existing ion sieve materials used as lithium ion adsorption materials in salt baths, the inventors found that although the existing ion sieve materials can selectively absorb lithium ions, it is difficult to release lithium ions after absorbing lithium ions, and thus it is difficult to achieve lithium ion recovery and to re-process the recovered lithium ions into reusable raw materials. In other words, it is difficult for existing ion sieve materials to achieve efficient recycling of lithium ions.

[0007] The concept of recycling and reuse is a green concept that meets the requirements of sustainable development. As a material closely related to daily life, lithium plays an extremely important role in the energy industry, aerospace industry, metal smelting and manufacturing industry, refrigeration, ceramics, glass and other industries. Therefore, how to effectively solve the problem of salt bath "poisoning" while achieving efficient recycling of lithium ions has become the key problem that the inventors want to solve.

[0008] In order to effectively solve the problem of salt bath "poisoning" in the process of manufacturing chemically strengthened glass and realize efficient recovery of lithium ions, the present application provides a method for manufacturing an ion sieve and chemically strengthened glass.

[0009] Specifically, the following technical solutions are provided:

[0010] In a first aspect, an ion sieve is provided, which comprises, expressed in terms of molar percentage of oxides: SiO 2 20.00~50.00mol%Al 2 O 3 2.00~20.00mol%B 2 O 3 0.00~15.00mol% and Na 2 O 40.00~70.00mol%;

[0011] Wherein, the composition of the ion sieve satisfies the following relationship, measured in terms of the content expressed as a molar percentage of the oxide:

[0012] 40.00mol%≤SiO 2 +Al 2 O 3 +B 2 O 3 ≤55.00mol%;

[0013] 0<(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <0.40;

[0014] 0.35<Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <1.85.

[0015] In some embodiments of the present application, the composition of the ion sieve satisfies the following relationship, expressed in terms of the content expressed as a molar percentage of the oxide: 0.80≤Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )≤1.90, and / or,

[0016] Al 2 O 3 / Na 2 O = 0.05 to 0.35, and / or

[0017] 0.50<Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <1.50.

[0018] In some embodiments of the present application, the SiO 2 The molar percentage is 25.00 to 50.00 mol%, preferably 30.00 to 50.00 mol%, more preferably 30.00 to 45.00 mol%; and / or,

[0019] The Na 2 The molar percentage of O is 40.00 to 65.00 mol%, preferably 45.00 to 65.00 mol%, and more preferably 45.00 to 55.00 mol%;

[0020] and / or,

[0021] The Al 2 O 3 The molar percentage is 3.00 to 20.00 mol%, preferably 4.00 to 15.00 mol%;

[0022] and / or,

[0023] B 2 O 3 The molar percentage is 0.00 to 10.00 mol%, preferably 0.00 to 5.00 mol%.

[0024] In some embodiments of the present application, 100 wt% NaNO 3 Based on the mass of the molten salt bath, 1 wt% of the ion sieve is added to 100 wt% NaNO containing 800 ppm-1000 ppm of lithium ions. 3 In a molten salt bath, after reacting at 500° C. for 12 hours, the absorption rate of the ion sieve for lithium ions is ≥55.00%, preferably ≥60.00%, and / or,

[0025] Based on the mass of the molten salt bath, 1wt% of the ion sieve is added to a molten salt bath containing 10ppm-200ppm of lithium ions. After reacting at 500°C for 12 hours, the absorption rate of the ion sieve for lithium ions is ≥75%, preferably ≥80%, and / or,

[0026] The ion sieve is placed in a 5wt% HCl aqueous solution and soaked at 95°C for 18 hours, and the weight loss percentage of the ion sieve is ≥28.00%, preferably ≥30.00%, and more preferably ≥36.00%.

[0027] In some embodiments of the present application, the ion sieve is in a granular, sheet-like or porous form;

[0028] Preferably, the particle size of the granular ion sieve is 1 mm-4 mm; and / or,

[0029] The thickness of the sheet-like ion sieve is 0.3 mm-1.0 mm.

[0030] In a second aspect, a method for preparing the above-mentioned ion sieve is provided, comprising preparing materials according to the above-mentioned ion sieve formula components, and then performing a melting treatment, molding and cooling to obtain the ion sieve;

[0031] Preferably, the temperature of the melt treatment is 1000°C to 1650°C.

[0032] In a third aspect, there is provided an application of the ion sieve or the ion sieve prepared by the preparation method in the fields of recovering lithium from lithium-containing waste glass, recovering lithium from waste battery materials or manufacturing chemically strengthened glass.

[0033] In a fourth aspect, a method for recovering lithium from a molten salt bath for chemically strengthened glass manufacturing is provided, comprising the following steps:

[0034] (1) adding the lithium-containing glass to be chemically strengthened and the above-mentioned ion sieve or the ion sieve prepared by the above-mentioned preparation method into a molten salt bath for chemical strengthening, or adding the above-mentioned ion sieve or the ion sieve prepared by the above-mentioned preparation method into a molten salt bath containing lithium ions after chemical strengthening, and using the ion sieve to absorb the lithium ions released by the glass into the molten salt bath;

[0035] (2) subjecting the ion sieve having absorbed lithium ions in step (1) to an acid hydrolysis treatment, and filtering to obtain an acid hydrolysis solution;

[0036] (3) adding a first ion precipitant to the acid hydrolysis solution obtained in step (2) to precipitate the impurity aluminum ions in the acid hydrolysis solution, filtering, adding a second ion precipitant to the obtained filtrate to precipitate the lithium ions in the filtrate, filtering to obtain a reusable lithium-containing material.

[0037] In some embodiments of the present application, in the above method for recovering lithium from a molten salt bath for chemically strengthened glass production, the temperature of the molten salt bath is 310°C to 650°C, preferably 380°C to 650°C, and more preferably 400°C to 650°C;

[0038] Preferably, the chemical strengthening molten salt bath contains sodium ions;

[0039] Further preferably, the chemical strengthening molten salt bath contains 5 wt% to 100 wt% of a sodium salt, wherein the sodium salt includes at least one of sodium nitrate, sodium chloride and sodium sulfate, and preferably the sodium salt is sodium nitrate; and / or,

[0040] The added amount of the ion sieve is 0.1-20.0 wt % based on the mass of the molten salt bath for chemical strengthening.

[0041] In some embodiments of the present application, in the above-mentioned method for recovering lithium from a salt bath for chemically strengthened glass manufacturing, in step (2), the acid solution for acidolysis treatment includes an aqueous hydrochloric acid solution and / or an aqueous nitric acid solution;

[0042] Preferably, the concentration of the acid solution is not less than 5wt%; preferably, the temperature of the acid hydrolysis treatment is 25°C to 95°C; more preferably, the time of the acid hydrolysis treatment is 8 to 24h; and / or,

[0043] In step (3), the first ion precipitant is an alkaline solution, preferably the first ion precipitant is ammonia water; and / or,

[0044] The second ion precipitation agent is a soluble carbonate, and preferably the second ion precipitation agent is sodium carbonate.

[0045] In a fifth aspect, a method for manufacturing chemically strengthened glass is provided, comprising the steps of: adding the above-mentioned ion sieve or the ion sieve obtained by the above-mentioned preparation method to a molten salt bath for chemical strengthening of glass, and bringing lithium-containing glass into contact with the molten salt bath for ion exchange.

[0046] In some embodiments of the present application, in the method for manufacturing the chemically strengthened glass, the temperature of the molten salt bath is 310°C to 650°C, preferably 380°C to 650°C, and more preferably 400°C to 650°C;

[0047] Preferably, after the step of adding the ion sieve to the molten salt bath, the Li ion concentration in the molten salt bath is 500 ppm or less;

[0048] More preferably, the molten salt bath contains sodium ions; the molten salt bath is at least one of nitrate, sulfate and chloride, preferably the molten salt bath is nitrate; and / or,

[0049] The added amount of the ion sieve is 0.1-20.0 wt % based on the mass of the molten salt bath for chemical strengthening.

[0050] In some embodiments of the present application, in the method for manufacturing the chemically strengthened glass, the method for manufacturing the chemically strengthened glass further includes a step of recovering lithium from the ion sieve added to the molten salt bath after use through an acid hydrolysis treatment process and a separation treatment process.

[0051] Beneficial effects of this application:

[0052] The present application optimizes the composition of the ion sieve material to give it a specific structure, thereby having the performance advantages of high lithium ion absorption rate and easy acid hydrolysis. The ion sieve of the present application can efficiently absorb lithium ions in the salt bath during the manufacturing process of chemically strengthened glass, ensure the smooth progress of ion exchange, and avoid the problem of "poisoning" in the salt bath. At the same time, after the ion sieve material that absorbs lithium ions is taken out of the salt bath, the absorbed lithium ions can be released into the acid solution through a simple acid hydrolysis process, and then combined with a simple separation process, the lithium ions released into the solution can be prepared into a reusable lithium-containing material, thereby realizing efficient recovery of lithium ions. The process of lithium ion recovery achieved by the ion sieve of the present application is relatively simple, low cost, and the recovery process does not produce a large amount of waste liquid, which meets the strategic goal requirements of national sustainable development. DETAILED DESCRIPTION

[0053] In this application, unless otherwise specified in specific circumstances, the numerical ranges listed herein include upper and lower limits, and "above" and "below" include the endpoint values, as well as all integers and fractions within the range, and are not limited to the specific values ​​listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A; and / or B" means only A, or only B, or both A and B.

[0054] In this application, ppm is by weight.

[0055] In some specific embodiments of the present application, an ion sieve is provided, which comprises the following components expressed in terms of molar percentage of oxide:

[0056] 20.00 mol% to 50.00 mol% SiO 2 ,

[0057] 40.00 mol% to 70.00 mol% Na 2 Oh,

[0058] 2 mol% to 20.00 mol% Al 2 O 3 ,

[0059] 0.00 mol% to 15.00 mol% B 2 O 3 ,

[0060] Wherein, the composition of the ion sieve satisfies the following relationship, measured in terms of the content expressed as a molar percentage of the oxide:

[0061] 40.00mol%≤SiO 2 +Al 2 O 3 +B 2 O 3 ≤55.00mol%;

[0062] 0<(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <0.40;

[0063] 0.35<Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <1.85.

[0064] Next, the scope of each component (ingredient) of the ion sieve of the present application is explained.

[0065] In the ion sieve of the present application, SiO 2It is an essential component used to form the framework of the ion sieve network structure. Its content directly affects the structure of the ion sieve, and then affects the stability of the ion sieve network structure and the performance of adsorption performance. Therefore, in order to ensure the stability of the ion sieve network structure and better play the adsorption and impurity removal performance, in this application, SiO is preferably used in mol%. 2 The content of is 20.00 mol% to 50.00 mol%, more preferably 25.00 mol% to 50.00 mol%, further preferably 30.00 mol% to 45.00 mol%.

[0066] In some embodiments of the present application, the above-mentioned ion sieve may contain 20.00mol% to 50.00mol%, 22.00mol% to 48.00mol%, 24.00mol% to 47.00mol%, 25.00mol% to 45.00mol%, 26.00mol% to 43.00mol%, 28.00mol% to 40.00mol%, 30.00mol% to 50.00mol%, 20.00mol% to 30.00mol%, 40.00mol% to 50 ...25.00mol% to 45.00mol%, 26.00mol% to 43.00mol%, 28.00mol% to 40.00mol%, 25.00mol% to 45.00mol%, 26.00mol% to 43.00mol%, 28.00mol% to 40.00mol%, 25.00mol% to 45.00mol%, 25.00mol% to 45.00mol%, 25.00mol% to 45.00mol%, 25.00mol% to % to 50.00 mol%, 30.00 mol% to 48.00 mol%, 30.00 mol% to 46.00 mol%, 30.00 mol% to 44.00 mol%, 30.00 mol% to 45.00 mol%, 30.00 mol% to 42.00 mol%, 30.00 mol% to 40.00 mol%, 20.00 mol% to 38.00 mol%, 20.00 mol% to 36.00 mol% or 20.00 mol% to 34.00 mol% of SiO 2 In some embodiments, the ion sieve may include 20.00 mol%, 22.00 mol%, 24.00 mol%, 25.00 mol%, 26.00 mol%, 28.00 mol%, 30.00 mol%, 31.00 mol%, 32.00 mol%, 34.00 mol%, 35.00 mol%, 36.00 mol%, 38.00 mol%, 40.00 mol%, 41.00 mol%, 42.00 mol%, 44.00 mol%, 45.00 mol%, 46.00 mol%, 48.00 mol%, or 50.00 mol% of SiO 2 , or SiO within the numerical range formed by any two of the above specific values ​​as endpoints 2 It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the ion sieve with the desired performance of the present application can be obtained.

[0067] In the ion sieve of the present application, Na 2 O is a necessary component. Its content determines the content of alkali metal sodium ions that can be used for ion exchange, which will directly affect the adsorption effect of the ion sieve on the impurity lithium ions in the salt bath. 2 O will provide free oxygen, which will affect the structure of the ion sieve and the stability of the ion sieve network structure. 2 Too little O will easily lead to less absorption of impurity lithium ions by the ion sieve, while if Na 2 Too much O can easily lead to problems such as the inability to form the ion sieve. Therefore, in order to ensure better impurity removal effect and structural stability of the ion sieve, in this application, Na 2 The content of O is 40.00 mol% to 70.00 mol%, more preferably 40.00 mol% to 65.00 mol%, further preferably 45.00 mol% to 65.00 mol% or 45.00 mol% to 55.00 mol%.

[0068] In some embodiments of the present application, the above-mentioned ion sieve may contain a molar percentage of 40.00-70.00 mol%, 42.00-68.00 mol%, 45.00-65.00 mol%, 48.00-63.00 mol%, 50.00-69.00 mol%, 40.00-60.00 mol%, 60.00-70.00 mol%, 41.00-63.00 mol%, 40.0 0 to 61.00 mol%, 41.00 to 59.00 mol%, 42.00 to 55.00 mol%, 45.00 to 70.00 mol%, 49.00 to 65.00 mol%, 40.00 to 55.00 mol%, 41.00 to 50.00 mol%, 40.00 to 48.00 mol%, 41.00 to 45.00 mol%, or 41.00 to 65.00 mol% of Na 2 In some embodiments, the ion sieve may include 40.00 mol%, 41.00 mol%, 42.00 mol%, 43.00 mol%, 44.00 mol%, 45.00 mol%, 46.00 mol%, 47.00 mol%, 49.00 mol%, 50.00 mol%, 51.00 mol%, 52.00 mol%, 53.00 mol%, 55.00 mol%, 57.00 mol%, 59.00 mol%, 61.00 mol%, 63.00 mol%, 65.00 mol%, 66.00 mol%, 67.00 mol%, 69.00 mol%, or 70.00 mol% of Na 2O, or Na within the numerical range formed by any two of the above specific values ​​as endpoints 2 O. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the ion sieve with the desired performance of the present application can be obtained.

[0069] In the ion sieve of the present application, Al 2 O 3 It is beneficial to improve the strain point and Tg point of the ion sieve, which is beneficial for its use in high temperature environment. 2 O 3 It is also conducive to the formation of aluminum oxide tetrahedrons to widen the network channel, thereby increasing the absorption rate and degree of the ion sieve for impurity lithium ions, and better exerting the absorption performance of the ion sieve for impurity lithium ions. 2 O 3 The higher the content, the more stable the ion sieve network structure and the faster the ion sieve exchange rate. 2 O 3 This will make it difficult to form the ion sieve, and in the process of acid hydrolysis of the ion sieve to recover lithium ions, excessive Al in the ion sieve will 3+ Introducing it into the acid solution will interfere with the precipitation method to recover lithium ions, which will increase the removal of Al impurities in the acid solution. 3+ Therefore, in this application, Al is preferred in terms of mol%. 2 O 3 The content of is 2.00 mol% to 20.00 mol%, more preferably 4.00 mol% to 15.00 mol%.

[0070] In some embodiments of the present application, the ion sieve may contain 2.00-20.00 mol%, 3.00-18.00 mol%, 4.00-16.00 mol%, 6.00-15.00 mol%, 8.00-12.00 mol%, 10.00-20.00 mol%, 12.00-18.00 mol%, 4.00-15.00 mol%, 2.00-16.00 mol%, 2.00-14.00 mol%, 2.00-12.00 mol% or 2.00-10.00 mol% of Al 2 O 3 In some embodiments, the ion sieve may contain 2.00 mol%, 3.00 mol%, 4.00 mol%, 6.00 mol%, 8.00 mol%, 10.00 mol%, 12.00 mol%, 14.00 mol%, 15.00 mol%, 16.00 mol%, 18.00 mol%, or 20.00 mol% of Al. 2 O3 , or Al within the numerical range consisting of any two of the above specific values ​​as endpoints 2 O 3 It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the ion sieve with the desired performance of the present application can be obtained.

[0071] In the ion sieve of the present application, B 2 O 3 It is an optional component for forming the framework of the ion sieve network structure. 2 O 3 It can reduce the melting temperature and molding temperature of the ion sieve and reduce the thermal expansion coefficient. At the same time, add an appropriate amount of B 2 O 3 It can help improve the acid hydrolysis performance of the ion sieve and help to recover the lithium ions absorbed in the ion sieve. 2 O 3 The content of is 0.00 mol% to 15.00 mol%, preferably 0.00 to 10.00 mol%, more preferably 0.00 mol% to 5.00 mol%.

[0072] In some embodiments of the present application, the ion sieve may contain 0.00-15.00 mol%, 1.00-14.00 mol%, 2.00-13.00 mol%, 3.00-12.00 mol%, 4.00-10.00 mol%, 5.00-9.00 mol%, 6.00-8.00 mol%, 7.00-15.00 mol%, 0.00-7.00 mol%, 0.00-6.00 mol%, 8.00-12.00 mol%, 0.00-2.00 mol%, 0.00-6.00 mol%, 1.00-9.00 mol%, 2.00-8.00 mol%, 3.00-7.00 mol% or 0.00-5.00 mol% of B. 2 O 3 In some embodiments, the ion sieve may include 0.00 mol%, 1.00 mol%, 2.00 mol%, 3.00 mol%, 4.00 mol%, 5.00 mol%, 6.00 mol%, 7.00 mol%, 8.00 mol%, 9.00 mol%, 10.00 mol%, 11.00 mol%, 12.00 mol%, 13.00 mol%, 14.00 mol%, or 15.00 mol% of B 2 O 3, or B within the numerical range formed by any two of the above specific values ​​as endpoints 2 O 3 It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the ion sieve with the desired performance of the present application can be obtained.

[0073] In some embodiments of the present application, the composition of the ion sieve satisfies the following relationship, measured in terms of the content expressed as a molar percentage of the oxide:

[0074] 40.00mol%≤SiO 2 +Al 2 O 3 +B 2 O 3 ≤55.00mol%.

[0075] In some embodiments of the present application, the SiO 2 +Al 2 O 3 +B 2 O 3 The sum of the molar percentages of may be 40.00-55.00 mol%, 41.00-53.00 mol%, 42.00-51.00 mol%, 43.00-50.00 mol%, 44.00-48.00 mol%, 45.00-55.00 mol%, 40.00-45.00 mol%, 47.00-50.00 mol%, 40.00-54.00 mol%, 43.00-53.00 mol%, 45.00-52.00 mol%, 41.00-51.00 mol%, 49.00-52.00 mol%, 50.00-55.00 mol%, 52.00-55.00 mol%, or 53.00-55.00 mol%. In some embodiments, the SiO 2 +Al 2 O 3 +B 2 O 3The sum of the molar percentages may be 40.00mol%, 41.00mol%, 42.00mol%, 43.00mol%, 44.00mol%, 45.00mol%, 46.00mol%, 47.00mol%, 48.00mol%, 49.00mol%, 50.00mol%, 51.00mol%, 52.00mol%, 53.00mol%, 54.00mol% or 55.00mol%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the ion sieve with the desired performance of the present application can be obtained.

[0076] In some embodiments of the present application, the composition of the ion sieve satisfies the following relationship, measured in terms of the content expressed as a molar percentage of the oxide:

[0077] 0<(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <0.40;

[0078] In some embodiments of the present application, the above (Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 The value of can be 0.01 to 0.39, 0.05 to 0.38, 0.10 to 0.35, 0.15 to 0.30, 0.30 to 0.39, 0.01 to 0.15, 0.01 to 0.35, 0.25 to 0.39, 0.20 to 0.35, 0.01 to 0.25 or 0.01 to 0.20. In some embodiments, the above (Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 The value of can be 0.01, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35 or 0.39, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the ion sieve with the desired performance of the present application can be obtained.

[0079] In some embodiments of the present application, the composition of the ion sieve satisfies the following relationship, measured in terms of the content expressed as a molar percentage of the oxide:

[0080] 0.35<Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <1.85.

[0081] In some embodiments of the present application, the above-mentioned Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 The value of may be 0.36 to 1.84, 0.38 to 1.80, 0.40 to 1.70, 0.45 to 1.60, 0.55 to 1.50, 0.53 to 1.40, 0.36 to 1.30, 0.38 to 1.20, 0.40 to 1.84, 1.30 to 1.84, 0.50 to 1.50, 0.51 to 1.49, 0.60 to 1.84, 0.70 to 1.80, 0.80 to 1.74, 0.90 to 1.64, 1.00 to 1.84, 0.36 to 0.90 or 1.20 to 1.84. In some embodiments, the above Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 The value of can be 0.36, 0.37, 0.40, 0.50, 0.51, 0.60, 0.70, 0.71, 0.80, 0.90, 0.94, 1.00, 1.10, 1.20, 1.30, 1.40, 1.49, 1.50, 1.60, 1.70, 1.80 or 1.84, or a value in the numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the ion sieve with the desired performance of the application can be obtained.

[0082] The ion sieve of the present application satisfies the content range of each oxide by satisfying a specific oxide content relationship, such as satisfying 40.00 mol % ≤ SiO 2 +Al 2 O 3 +B 2 O 3 ≤55.00mol%; 0<

[0083] (Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <0.40;0.35<Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )-(Al 2 O 3 +1.1×B 2 O 3 ) / SiO 2 <1.85. On the one hand, it can ensure the structural stability of the ion sieve so that the ion sieve can better exert its excellent adsorption effect on lithium ions in a high-temperature salt bath. On the other hand, it can give the ion sieve the performance advantage of easy acid decomposition so that the ion sieve can efficiently release the absorbed lithium ions into the acid solution, thereby helping to better realize the recovery and reuse of lithium.

[0084] In some embodiments of the present application, the composition of the ion sieve satisfies the following relationship, expressed in terms of the content expressed as a molar percentage of the oxide: 0.80≤Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3 )≤1.90. By making the composition of the ion sieve satisfy this relationship, it is beneficial for the ion sieve to form a specific and stable network structure, and it can ensure that there are sufficient sodium ions in the network structure that can be used to participate in ion exchange, which is beneficial for the ion sieve to exert its excellent adsorption effect on lithium ions in a high-temperature salt bath.

[0085] In some embodiments of the present application, the above-mentioned Na 2 O / (SiO 2 +Al 2 O 3 +B 2 O 3) can be 0.80, 0.90, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80 or 1.90, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the ion sieve with the desired performance of the present application can be obtained.

[0086] In some embodiments of the present application, the composition of the ion sieve satisfies the following relationship, expressed in terms of the content expressed in mole percentage of the oxide: Al 2 O 3 / Na 2 O = 0.05 to 0.35. By making the composition of the ion sieve satisfy this relationship, it is beneficial to ensure the rate of ion exchange and better exert the absorption performance of the ion sieve on impurity lithium ions.

[0087] In some embodiments of the present application, the above Al 2 O 3 / Na 2 The value of O can be 0.05, 0.08, 0.10, 0.15, 0.18, 0.20, 0.25, 0.28, 0.30, 0.32 or 0.35, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the ion sieve with the desired performance of the present application can be obtained.

[0088] In some embodiments of the present application, based on the mass of the molten salt bath, the ion sieve with a mass proportion of 1wt% is added to a molten salt bath containing 800ppm-1000ppm of lithium ions. After reacting for 12 hours at 500°C, the absorption rate of the ion sieve to lithium ions is ≥55.00%, preferably ≥60.00%. In the present application, under the above test conditions, the absorption rate of the ion sieve to lithium ions can be 55% to 80.00%, 60.00% to 80.00%, 55.00% to 75.00% or 60.00% to 75.00%, etc. This shows that the ion sieve of the present application has an excellent absorption effect on lithium ions in a high-temperature salt bath. It should be noted that the type of molten salt bath used in the above test is not particularly limited, for example, as long as it contains alkali metal ions with a larger radius, such as sodium ions and / or potassium ions, for example, sodium nitrate and / or potassium nitrate.

[0089] In some embodiments of the present application, based on the mass of the molten salt bath, the ion sieve with a mass proportion of 1wt% is added to a molten salt bath containing 10ppm-200ppm of lithium ions. After reacting for 12 hours at 500°C, the absorption rate of the ion sieve to lithium ions is ≥75.00%, preferably ≥80.00%. In the present application, under the above test conditions, the absorption rate of the ion sieve to lithium ions can be 75% to 95.00%, 80.00% to 95.00%, 75.00% to 85.00% or 80.00% to 95.00%, etc. This shows that the ion sieve of the present application has an excellent absorption effect on lithium ions in a high-temperature salt bath. It should be noted that the type of molten salt bath used in the above test is not particularly limited, for example, as long as it contains alkali metal ions with a larger radius, such as sodium ions and / or potassium ions, for example, sodium nitrate and / or potassium nitrate.

[0090] In some embodiments of the present application, the ion sieve is placed in a 5wt% HCl aqueous solution, and after soaking for 18 hours at 95°C, the weight loss percentage of the ion sieve is ≥28.00%, preferably ≥30.00%, and more preferably ≥36.00%. In the present application, under the above test conditions, the weight loss percentage of the ion sieve can be 28.00% to 70.00%, 30.00% to 70.00%, 28.00% to 65.00% or 30.00% to 65.00%, etc. This shows that the ion sieve of the present application has the performance of easy acid decomposition, which is conducive to releasing a large amount of lithium ions absorbed in the ion sieve into the acid solution.

[0091] The present application provides a method for preparing the above-mentioned ion sieve, comprising the following steps: weighing the raw materials of each component according to the proportion of the ion sieve formula components and mixing them evenly, melting the resulting mixture, and then molding and cooling the resulting molten liquid to make an ion sieve. Wherein, the molding process includes but is not limited to, the molten liquid can be rolled or drawn into a sheet-like ion sieve by an external force, or the molten liquid can be poured into water for quenching or air cooling to obtain a granular ion sieve, or a porous ion sieve substrate can be made by adding a foaming agent to the molten liquid. There is no special restriction on the foaming agent, as long as it can achieve a foaming effect to make a porous ion sieve.

[0092] In the preparation method of the ion sieve provided in the present application, the raw materials of each component are mixed evenly and then melt-treated at 1000° C. to 1650° C. to obtain a liquid melt.

[0093] In the preparation method of the above-mentioned ion sieve provided in the present application, when the granular ion sieve is formed by water quenching, the water quenching temperature can be 10°C to 80°C, for example, it can be 10°C, 15°C, 20°C, 22°C, 25°C, 30°C, 35°C, 45°C, 50°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc., and the size of the ion sieve particles is controlled by controlling the temperature so that the ion sieve particles meet the particle size of 1mm to 10mm, for example, the particle size of the granular ion sieve can be 1mm, 1.5mm, 2mm, 2.5mm, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm or 10mm, etc. The particle size of the granular ion sieve is preferably between 2mm and 5mm. It should be noted that the "particle size" here refers to the maximum diameter size of the granular ion sieve.

[0094] In the preparation method of the ion sieve provided in the present application, when the granular ion sieve is formed by air cooling, it can be sieved with an 18-mesh or 5-mesh metal wire mesh test sieve to obtain a granular ion sieve with a particle size of 1 mm to 4 mm.

[0095] In the preparation method of the above-mentioned ion sieve provided in the present application, when the sheet-like ion sieve is rolled or drawn by external force, the thickness of the sheet-like ion sieve can be 0.3mm to 1.0mm, for example, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm or 1.0mm, etc. Preferably, the thickness of the sheet-like ion sieve is 0.4mm to 0.6mm. The sheet-like ion sieve here can be an irregular sheet, the shortest side of which can be at least 0.3cm, and the largest / longest side can be less than 10cm.

[0096] Since the ion sieve material of the present application has excellent lithium ion adsorption effect and the performance advantages of easy acid decomposition, it can be applied to the recovery of lithium from lithium-containing waste glass, recovery of lithium from waste battery materials, recovery of lithium from salt baths for chemical strengthening of glass, and application in the field of chemically strengthened glass manufacturing, used to control the lithium ion concentration in the salt bath, avoid the "poisoning" phenomenon of the salt bath, and be used to efficiently recover lithium and realize the recycling and reuse of lithium. The waste battery material referred to in the present application is waste battery material containing lithium.

[0097] The present application provides a method for recovering lithium from a molten salt bath for chemically strengthened glass manufacturing, comprising the following steps:

[0098] (1) adding the lithium-containing glass to be chemically strengthened and the above-mentioned ion sieve or the ion sieve prepared by the above-mentioned preparation method into a molten salt bath for chemical strengthening, or adding the above-mentioned ion sieve or the ion sieve prepared by the above-mentioned preparation method into a molten salt bath containing lithium ions after chemical strengthening, and using the ion sieve to absorb the lithium ions released by the glass into the molten salt bath;

[0099] (2) subjecting the ion sieve having absorbed lithium ions in step (1) to an acid hydrolysis treatment, and filtering to obtain an acid hydrolysis solution;

[0100] (3) adding a first ion precipitant to the acid hydrolysis solution obtained in step (2) to precipitate the impurity aluminum ions in the acid hydrolysis solution, filtering, adding a second ion precipitant to the obtained filtrate to precipitate the lithium ions in the filtrate, filtering to obtain a reusable lithium-containing material.

[0101] In some embodiments of the present application, in the above method for recovering lithium from a molten salt bath for chemically strengthened glass production, the temperature of the molten salt bath is 310°C to 650°C, preferably 380°C to 650°C, and more preferably 400°C to 650°C;

[0102] Preferably, the chemical strengthening molten salt bath contains sodium ions;

[0103] Further preferably, the chemical strengthening molten salt bath contains 5wt% to 100wt% of sodium salt, for example, it may contain 5wt% to 100wt%, 5wt% to 30wt%, 30wt% to 100wt%, 5wt% to 60wt%, 30wt% to 70wt%, 30wt% to 50wt% or 60wt% to 100wt% of sodium salt. The sodium salt includes at least one of sodium nitrate, sodium chloride and sodium sulfate, and preferably the sodium salt is sodium nitrate. For example, in some embodiments, the chemical strengthening molten salt bath may contain 5wt%, 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 80wt% or 100wt% of sodium nitrate, or sodium nitrate within a numerical range consisting of any two of the above specific numerical values ​​as endpoints; and / or,

[0104] The added amount of the ion sieve is 0.1-20.0 wt % based on the mass of the molten salt bath for chemical strengthening.

[0105] In some embodiments of the present application, in the above-mentioned method for recovering lithium from a salt bath for chemically strengthened glass manufacturing, in step (2), the acid solution for acidolysis treatment includes an aqueous hydrochloric acid solution and / or an aqueous nitric acid solution;

[0106] Preferably, the concentration of the acid solution is not less than 5wt%; preferably, the temperature of the acid hydrolysis treatment is 25°C to 95°C; more preferably, the time of the acid hydrolysis treatment is 8 to 24h; and / or,

[0107] In step (3), the first ion precipitant is an alkaline solution, preferably the first ion precipitant is ammonia water; and / or,

[0108] The second ion precipitation agent is a soluble carbonate, and preferably the second ion precipitation agent is sodium carbonate.

[0109] The present application provides a method for manufacturing chemically strengthened glass, comprising the following steps: a step of adding the above-mentioned ion sieve into a molten salt bath for chemically strengthening glass, and a step of bringing lithium-containing glass into contact with the molten salt bath to perform ion exchange.

[0110] In the present application, the above-mentioned ion sieve and the lithium-containing glass to be chemically strengthened can be added to the molten salt bath together (to achieve the goal that during the ion exchange process of the glass, the ion sieve simultaneously absorbs the lithium ions released from the glass in the molten salt bath), or the above-mentioned ion sieve can be added to the molten salt bath after the lithium-containing glass is chemically strengthened (for example, after the glass ion exchange is completed, the strengthened glass is taken out of the molten salt bath, and the ion sieve is added to the molten salt bath to absorb lithium ions).

[0111] In the present application, the ion sieve added to the molten salt bath will absorb the lithium ions released from the glass into the molten salt bath after the lithium-containing glass and the molten salt bath undergo Li-Na exchange (lithium ions in the glass are exchanged with sodium ions in the salt bath). Specifically, the sodium ions in the ion sieve will be exchanged with the lithium ions in the molten salt bath, thereby achieving control of the lithium ion concentration in the molten salt bath, ensuring the recovery of the composition and properties of the molten salt bath, and avoiding the problem of "poisoning" of the salt bath during the manufacturing process of chemically strengthened glass.

[0112] The present application uses the above-mentioned ion sieve material in the process of manufacturing chemically strengthened glass, which can efficiently and selectively absorb the lithium ions released by the lithium-containing glass during the chemical strengthening process, reduce the lithium ion content in the molten salt bath, and prevent the "poisoning" of the molten salt bath. At the same time, based on the performance advantage of the ion sieve being easy to acid-lyze, it is easy to release the absorbed lithium ions into the acid solution, thereby easily realizing the efficient recycling of lithium ions.

[0113] In some embodiments of the present application, after the step of adding the ion sieve to the molten salt bath, the Li ion concentration in the molten salt bath is 500 ppm or less, preferably 100 ppm or less.

[0114] In the present application, the amount of Na ions that can be used for ion exchange in the ion sieve added to the molten salt bath will gradually decrease as the strengthening time increases, that is, as the strengthening time increases, the absorption effect of the ion sieve on lithium ions will decrease. Therefore, in this case, it is preferred to remove the ion sieve from the molten salt bath and add new ion sieve materials to the salt bath. That is, in some embodiments of the present application, the method for manufacturing the chemically strengthened glass further includes the step of removing the ion sieve that has absorbed lithium ions from the molten salt bath and the step / process of adding new ion sieves to the salt bath.

[0115] It should be noted that when the ion sieve is added to the molten salt bath together with the glass, the time for the ion sieve to absorb lithium ions in the salt bath refers to the time from when the glass starts to be strengthened to when the ion sieve is taken out from the molten salt bath.

[0116] In some embodiments of the present application, the amount of ion sieve added to the molten salt bath is not particularly limited and can be appropriately adjusted according to the total amount of the molten salt bath composition, the content of lithium ions, the desired treatment time, etc. In some embodiments, the amount of ion sieve added includes but is not limited to 0.1-20.0wt% based on the mass of the molten salt bath.

[0117] In some embodiments of the present application, the temperature of the molten salt bath is 310° C. to 650° C., preferably 380° C. to 650° C., and more preferably 400° C. to 650° C. The type of the molten salt bath is not particularly limited as long as it contains large alkali metal ions (e.g., sodium ions and / or potassium ions).

[0118] In some embodiments of the present application, the molten salt bath contains sodium ions. In some embodiments of the present application, the molten salt bath is at least one of nitrates, sulfates and chlorides, preferably the molten salt bath is a nitrate, for example, sodium nitrate and / or potassium nitrate. In some embodiments of the present application, the molten salt bath may contain 5wt% to 100wt%, 30wt% to 100wt%, 60wt% to 100wt%, 5wt% to 60wt%, 30wt% to 60wt%, 30wt% to 90wt% or 5wt% to 30wt% of a sodium salt, the sodium salt may include at least one of sodium nitrate, sodium chloride and sodium sulfate, preferably the sodium salt is sodium nitrate, more preferably the molten salt bath is 100wt% of sodium nitrate.

[0119] In the present application, the lithium-containing glass is brought into contact with the molten salt bath (e.g., the lithium-containing glass is immersed in the molten salt bath) to perform ion exchange, that is, the glass is chemically strengthened by the ion exchange method. During the ion exchange process, the smaller alkali metal lithium ions in the lithium-containing glass are replaced or "exchanged" by larger alkali metal ions with the same valence state close to the glass, and the larger ions replace the smaller ions to construct a compressive stress layer in the glass. The ion exchange strengthening method can be carried out in multiple steps (e.g., two-step ion exchange) or in a single step. The ion exchange process may include, but is not limited to: immersing the glass in a single salt bath, or immersing it in multiple salt baths with the same or different compositions, and washing and / or annealing steps may be provided between immersions. In the present application, other monovalent metal ions, such as Ag + 、Tl + , Cu + Etc., can also be used to exchange monovalent ions in glass.

[0120] In some embodiments of the present application, before the chemical strengthening treatment, the glass may be preheated at 300 to 400° C. as required, and the preheating time is preferably 10 to 30 minutes.

[0121] In some embodiments of the present application, a thermal migration process at 350 to 500° C. may be performed between multiple strengthening steps as needed, and the thermal migration time is preferably 15 to 120 minutes.

[0122] In the present application, lithium-containing glass is a glass material that contains lithium, can be formed, and can be strengthened by chemical strengthening treatment. Various glasses can be used, for example, ordinary lithium aluminum silicate glass, microcrystalline glass containing microcrystalline phase, etc.

[0123] In the present application, there is no particular restriction on the thickness and shape of the lithium-containing glass. The lithium-containing glass may be in various shapes, such as a flat plate with uniform thickness, a shape with a curved surface on at least one of the front and back surfaces, and a three-dimensional shape with a curved portion. In addition, the glass may be processed according to the shape of the intended use, such as mechanical processing such as cutting, end surface processing, and hole processing. As a specific shape of the lithium-containing glass, for example, a plate with a thickness of 0.3 mm to 2.0 mm can be cited.

[0124] In some embodiments of the present application, the method for manufacturing the chemically strengthened glass further includes a step of recovering lithium from the ion sieve added to the molten salt bath after use through an acid hydrolysis treatment process and a separation treatment process.

[0125] In some embodiments of the present application, the acid hydrolysis treatment process includes: placing the ion sieve in an acid solution for acid hydrolysis. The acid solution used for acid hydrolysis can be a strong acid aqueous solution. Preferably, the acid solution includes a hydrochloric acid aqueous solution and / or a nitric acid aqueous solution. In order to efficiently release the lithium ions absorbed in the ion sieve into the acid solution, preferably, the concentration of the acid solution is not less than 5wt%, for example, the concentration of the acid solution can be 5wt% to 15wt%. In order to accelerate the acid hydrolysis rate of the ion sieve, preferably, the temperature of the acid solution is 25°C to 95°C; preferably, the acid hydrolysis time is 8 to 24h.

[0126] In order to improve the purity of recovered lithium, before the acid hydrolysis process, the ion sieve may be soaked in deionized water for 30 minutes and then rinsed with running water and dried to remove the molten salt attached to the surface of the ion sieve.

[0127] In some embodiments of the present application, the separation process includes: filtering the mixed solution obtained by acid hydrolysis and the undissolved ion sieve to obtain an acid hydrolysis solution and undissolved matter, adding a first ion precipitant to the acid hydrolysis solution, filtering to remove aluminum ion impurities in the acid hydrolysis solution, and then adding a second ion precipitant to the filtrate to recover and obtain a reusable lithium-containing material. Preferably, the first ion precipitant is an alkaline solution, preferably the first ion precipitant is ammonia water; preferably, the second ion precipitant is a soluble carbonate, preferably the second ion precipitant is sodium carbonate.

[0128] The technical solution of the present application is described in detail below through preparation examples and application examples.

[0129] 1: Specific operation examples

[0130] Preparation Example S1

[0131] <Preparation of ion sieve>

[0132] According to the component ratio of the ion sieve formula 1 of S1 in Table 1, the raw materials (conventional industrial raw materials) are configured in a platinum crucible, and the total amount of the configured raw materials is 1000 g. Then, a V-type mixer is used to mix for 30 minutes. After mixing, the resulting mixture is melted. Specifically, the platinum crucible is heated to 1500°C and kept at this temperature for 3 hours. The resulting mixture is stirred until it is molten to form a molten liquid.

[0133] The molten liquid was poured onto a 200° C. hot plate for air cooling, and after cooling, it was sieved with 18-mesh and 10-mesh metal wire woven mesh test sieves to obtain a granular ion sieve material with a particle size of 1 mm to 2 mm.

[0134] <Application test of lithium ion absorption rate of ion sieve>

[0135] The prepared ion sieve was placed in a molten salt bath at 500°C for testing. The amount of ion sieve used was 1.00wt% of the weight of the molten salt bath, and the total test time was 12.0h. The lithium ion concentration in the salt bath was tested before and after the addition of the ion sieve, and the absorption rate of the ion sieve for lithium ions in the salt bath was calculated.

[0136] Ion sieve absorption rate of lithium ions = (C 1 -C 2 ) / C 1 ;

[0137] C 1 ——Lithium ion concentration in the salt bath before the test, ppm;

[0138] C 2 ——Lithium ion concentration in the salt bath after the test, ppm.

[0139] Preparation method of the molten salt bath for the test: Sodium nitrate is taken, and 1wt% of lithium nitrate (to provide lithium ions) is added to the sodium nitrate to obtain a mixed salt, and the mixed salt is melted to prepare a molten salt bath for the test. For example, if 1kg of sodium nitrate is taken, 10g of lithium nitrate is added to prepare a molten salt bath.

[0140] <Carry out the ion sieving acid hydrolysis test and lithium ion concentration test according to the following method>

[0141] 1) Ion sieve acid hydrolysis test method

[0142] Weigh 20 g of ion sieve and add it to 200 ml of 5 wt % HCl aqueous solution. Acid hydrolyze it at 95° C. for 18 h. Filter out the undissolved ion sieve, then wash it with water, dry it, weigh it, and calculate the weight loss percentage of the ion sieve before and after acid hydrolysis.

[0143] Acid hydrolysis weight loss percentage = (m 1 -m 2 ) / m 1 ;

[0144] m 1 ——Weight of ion sieve before acid hydrolysis, g;

[0145] m 2 ——Weight of ion sieve after acid hydrolysis, g.

[0146] 2) Test method for lithium ion concentration in salt bath

[0147] The concentration of lithium ions in the salt bath was tested using an atomic absorption spectrophotometer AA-6880.

[0148] Specifically, an appropriate amount of molten salt bath with a lithium ion concentration to be measured is taken out from the strengthening furnace. After the molten salt bath is cooled, 0.25 g of the cooled solid substance is accurately weighed into a 100 ml glass beaker, and an appropriate amount of deionized water is added to dissolve it. The solid substance is then filtered into a 100 ml volumetric flask with slow filter paper to obtain a solution to be tested.

[0149] Use a pipette to draw 1 ml of the solution to be tested into a 100 ml volumetric flask, and add 1 ml of hydrochloric acid aqueous solution into the volumetric flask (the preparation method of the hydrochloric acid aqueous solution: according to the volume ratio, use high-grade pure 36-38wt% hydrochloric acid produced by Chongqing Wansheng Chuandong Chemical Group Co., Ltd.: deionized water = 1:1, mix and shake to prepare the hydrochloric acid aqueous solution), then add deionized water to the volumetric flask to make up the volume, shake well, and use an atomic absorption spectrophotometer to test the concentration of lithium ions in the salt bath using the corresponding standard curve.

[0150] 3) Testing method for lithium ion concentration in the filtrate obtained after acid hydrolysis of ion sieve

[0151] Use a pipette to draw 1 ml of the test solution (the filtrate after the ion sieving acid hydrolysis experiment) into a 100 ml volumetric flask, and add 1 ml of hydrochloric acid aqueous solution to the volumetric flask (the preparation method of the hydrochloric acid aqueous solution: according to the volume ratio, use high-grade pure 36-38wt% hydrochloric acid produced by Chongqing Wansheng Chuandong Chemical Group Co., Ltd.: deionized water = 1:1, mix and shake to prepare the hydrochloric acid aqueous solution), then add deionized water to the volumetric flask to make up the volume, shake well, and use an atomic absorption spectrophotometer to test the concentration of lithium ions in the test solution using the corresponding standard curve.

[0152] 4) Al in the filtrate obtained after acid hydrolysis of the ion sieve 2 O 3 Concentration test method

[0153] Use a pipette to draw 1 ml of the test solution (the filtrate after the ion sieving acid hydrolysis experiment) into a 250 ml glass beaker, add 25 ml of 0.01 mol / LEDTA standard solution, heat to above 60 ° C, and adjust the pH of the test solution to 3.5-4.0 (test with precision pH test paper) with ammonia solution (1:1) and sulfuric acid aqueous solution (according to the volume ratio, sulfuric acid: deionized water = 1:1, mix and shake to obtain sulfuric acid aqueous solution). Use a glass rod to press a small piece of filter paper (to prevent violent boiling), cover with a watch glass and heat until boiling, then turn to low heat and continue heating for 5 minutes, then cool to room temperature, rinse the watch glass and the cup wall with deionized water, add 6ml 20wt% hexamethylenetetramine solution (adjust pH to 5.5-6), add 0.15ml xylenol orange indicator, add 0.1ml sulfuric acid aqueous solution (according to the volume ratio, sulfuric acid: deionized water = 1:1, mix and shake to prepare sulfuric acid aqueous solution), until the solution turns bright yellow, use 0.01mol / L zinc acetate standard solution to back-titrate until the solution changes from bright yellow to stable rose red as the end point, calculate the Al in the test solution by the volume of 0.01mol / L zinc acetate standard solution consumed 2 O 3 concentration.

[0154]

[0155] C(Al 2 O 3 ) is the Al content of the solution to be tested 2 O 3 The mass concentration is in mg / ml;

[0156] T 2 0.01mol / L EDTA standard solution for Al 2 O 3 The titer (the mass of the component to be tested equivalent to 1 ml of standard solution) is expressed in milligrams per milliliter (mg / ml). 2It is 0.52mg / ml.

[0157] a is the volume ratio of 0.01 mol / L zinc acetate standard solution to EDTA standard solution.

[0158] Among them, the calibration method of the volume ratio of 0.01mol / L zinc acetate standard solution to 0.01mol / L EDTA standard solution is as follows: accurately aspirate 10ml of 0.01mol / L EDTA standard solution, place it in a 250ml beaker, dilute it to 100ml with water, add 6ml of 20wt% hexamethylenetetramine solution to adjust the pH to 5.7, add 0.15ml of xylenol orange indicator, and titrate with 0.01mol / L zinc acetate standard solution until the solution changes from yellow to stable rose red as the end point.

[0159]

[0160] V is the volume of 0.01 mol / L zinc acetate standard solution consumed during titration, in milliliters (ml);

[0161] V 2 The volume of 0.01 mol / L zinc acetate standard solution consumed by the test solution, in milliliters (ml);

[0162] V EDTA is the volume of 0.01 mol / L EDTA standard solution added, in milliliters (ml);

[0163] V 测 The volume of the solution to be tested is in milliliters (ml).

[0164] Preparation Examples S2-S4 and Preparation Examples D1-D4 were carried out under the same operating conditions as Preparation Example S1, except that the formulation compositions of the ion sieves shown in Table 1 were different.

[0165] Preparation Examples D5-D11

[0166] The same operation conditions as those of Preparation Example S1 were used, except that the formulations for preparing the ion sieves shown in Table 2 were different.

[0167] Table 1 Ion sieve formula of Preparation Examples S1-S4 and Preparation Examples D1-D4

[0168]

[0169]

[0170] Table 2 Ion sieve formulations for preparation examples D5-D11

[0171]

[0172] The acid hydrolysis weight loss percentage and lithium ion absorption rate of the ion sieves prepared in Preparation Examples S1-S4 and Preparation Examples D1-D11 were tested according to the above method. The results are shown in Table 3.

[0173] Table 3 Test results of Preparation Examples S1-S4 and Preparation Examples D1-D11

[0174] serial number Acid hydrolysis weight loss percentage, % Absorption rate of lithium ions by ion sieve, % Preparation Example S1 30.90 62.78 Preparation Example S2 39.40 68.84 Preparation Example S3 40.90 70.62 Preparation Example S4 49.60 63.16 Preparation Example D1 25.10 61.29 Preparation Example D2 47.44 50.21 Preparation Example D3 19.30 45.05 Preparation Example D4 17.73 42.05 Preparation Example D5 28.66 45.88 Preparation Example D6 32.36 40.92 Preparation Example D7 61.58 34.64 Preparation Example D8 15.12 41.40 Preparation Example D9 18.11 41.44 Preparation Example D10 29.02 46.44 Preparation Example D11 35.05 37.03

[0175] As shown in Table 3, the acid hydrolysis weight loss percentage of the ion sieves prepared in the preparation examples S1-S4 of the present application is 30.9%-49.6%, reaching more than 30%, and the absorption rate of lithium ions is 62.78%-70.62%, exceeding 60%. Although the lithium ion absorption rate of the preparation example D1 can reach 61.29%, the acid hydrolysis weight loss percentage is only 25.10%, less than 30%; the acid hydrolysis weight loss percentages of the preparation examples D2, D6, D7, and D11 are all more than 30%, but the lithium ion absorption rates are all less than 55%.

[0176] Application Example 1

[0177] This experiment is an application test to test the effect of ion sieve in absorbing and recovering lithium.

[0178] The ion sieves prepared in Preparation Examples S2 and S3 and Preparation Examples D3 and D4 were respectively taken, and a lithium ion absorption experiment was first performed according to the experimental conditions in Table 4. Then, the ion sieves after the lithium ion absorption test were acid-hydrolyzed, and the filtrate obtained after the acid hydrolysis was subjected to an aluminum removal operation to obtain a lithium ion-containing solution. The results are shown in Table 4.

[0179] Table 4

[0180]

[0181]

[0182] As shown in Table 4, the absorption and recovery effects of the ion sieve of the present application on lithium ions are investigated by using lithium nitrate as the source of lithium ions. When the ion sieves prepared in Example S2 and S3 are added in an amount of 1wt%, the absorption rates of lithium ions are 68.84% and 70.62% respectively, and the release rates of lithium ions after acid hydrolysis treatment of the ion sieves are 93.88% and 92.81% respectively, and the recovery rates of lithium ions are 63.27% and 63.83% respectively. When the ion sieves prepared in Example D3 and D4 are added in an amount of 1wt%, the absorption rates of lithium ions are 45.05% and 42.05% respectively, and the release rates of lithium ions after acid hydrolysis treatment of the ion sieves are 76.17% and 66.70% respectively, and the recovery rates of lithium ions are 32.78% and 27.52% respectively. It can be seen that the ion sieves prepared in Example S2 and S3 are significantly improved in terms of absorption rate, release rate of lithium ions and recovery rate.

[0183] At the same time, it can be seen from Table 4 that as the amount of the ion sieve prepared in Preparation Example S3 increases, the absorption rate of lithium ions also increases.

[0184] Application Example 2

[0185] This experiment is an application test of ion sieve in the manufacture of chemically strengthened glass.

[0186] Three groups of experiments were designed in this experiment. Five pieces of glass A (size: 50mm*50mm*0.7mm) were selected in each group (in terms of molar percentage of oxides, the composition of glass A contains: 69.2mol% SiO 2 、4.22mol%Al 2 O 3 、0.95mol%P 2 O 5 、1.70mol%ZrO 2 、1.58mol%Na 2 O, 20.73 mol% Li 2 O and 1.62 mol% B 2 O 3 ) were subjected to chemical strengthening treatment. In two experiments, ion sieves were added to the molten salt bath, and in one experiment, no ion sieves were added. The chemical strengthening treatment was a single-step strengthening treatment. The molten salt bath for chemical strengthening was 100 wt% NaNO at 500 °C. 3 .

[0187] The three groups of experiments are:

[0188] (1) Blank group: no ion sieve was added to the molten salt bath;

[0189] (2) Control group: Based on the mass of the molten salt bath, 1 wt% of the ion sieve prepared in Preparation Example D3 was added to the molten salt bath;

[0190] (3) Experimental group: Based on the mass of the molten salt bath, 1 wt % of the ion sieve prepared in Preparation Example S2 was added to the molten salt bath.

[0191] During the chemical strengthening process of glass A, the lithium ion concentration in the molten salt bath was tested at regular intervals. The results are shown in Table 5.

[0192] Table 5

[0193]

[0194]

[0195] As shown in Table 5, with the increase of strengthening time, the lithium ion concentration in the molten salt bath of the blank group without adding ion sieve gradually increased; while the lithium ion concentration in the molten salt bath of the control group and the experimental group was significantly lower than that of the blank group during the strengthening process after adding ion sieve to the molten salt bath, which indicates that the ion sieve absorbed the lithium ions released by the glass in the molten salt bath during the chemical strengthening of glass A. Compared with the control group, the lithium ion concentration in the molten salt bath of the experimental group increased slowly, which well controlled the concentration of lithium ions in the molten salt bath, ensured the composition and performance of the molten salt bath, and effectively avoided the problem of salt bath "poisoning" in the manufacturing process of chemically strengthened glass.

[0196] In summary, the present application optimizes the composition of the ion sieve material to give it a specific structure, thereby having the performance advantages of high lithium ion absorption rate and easy acid decomposition. It can be used to recover lithium from lithium-containing waste glass, recover lithium from waste battery materials, or recover lithium from salt baths for chemical strengthening of glass, as well as in the field of chemically strengthened glass manufacturing, to control the lithium ion concentration in the salt bath, to avoid the "poisoning" phenomenon of the salt bath, to efficiently recover lithium, and to achieve lithium recycling and reuse.

[0197] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solution of the present application rather than to limit it. Although the present application has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present application.

Claims

1. An ion sieve for absorbing lithium ions, characterized in that: Expressed in terms of molar percentage of oxides, its composition contains: SiO2 20.00-50.00 mol%, Al2O3 4.00-20.00 mol%, B2O3 0.00-15.00 mol% and Na2O4 0.00-70.00 mol%; Wherein, the composition of the ion sieve satisfies the following relationship, measured in terms of the content expressed as a molar percentage of the oxide: 40.00mol%≤SiO2+Al2O3+B2O3≤55.00mol%; 0<(Al2O3+1.1×B2O3) / SiO2<0.40; 0.35<Na2O / (SiO2+Al2O3+B2O3)-(Al2O3+1.1×B2O3) / SiO2<1.

85.

2. The ion sieve for absorbing lithium ions according to claim 1, characterized in that: The composition of the ion sieve satisfies the following relationship, expressed in terms of the content expressed as a molar percentage of the oxide: 0.80≤Na2O / (SiO2+Al2O3+B2O3)≤1.90; and / or, Al2O3 / Na2O=0.05~0.35; and / or, 0.50<Na2O / (SiO2+Al2O3+B2O3)-(Al2O3+1.1×B2O3) / SiO2<1.

50.

3. The ion sieve for absorbing lithium ions according to claim 1, characterized in that: The molar percentage of SiO2 is 25.00-50.00 mol%; and / or, The molar percentage of Na2O is 40.00-65.00 mol%; and / or, The molar percentage of Al2O3 is 10.00-20.00 mol%; and / or, The molar percentage of B2O3 is 0.00 to 10.00 mol%.

4. The ion sieve for absorbing lithium ions according to claim 1, characterized in that: The molar percentage of SiO2 is 30.00-50.00 mol%; and / or, The molar percentage of Na2O is 45.00-65.00 mol%; and / or, The molar percentage of Al2O3 is 4.00-15.00 mol%; and / or, The molar percentage of B2O3 is 0.00 to 5.00 mol%.

5. The ion sieve for absorbing lithium ions according to claim 3, characterized in that: The molar percentage of SiO2 is 30.00-45.00 mol%; and / or, The molar percentage of the Na2O is 45.00-55.00 mol%.

6. The ion sieve for absorbing lithium ions according to claim 2, characterized in that: The molar percentage of SiO2 is 25.00-50.00 mol%; and / or, The molar percentage of Na2O is 40.00-65.00 mol%; and / or, The molar percentage of Al2O3 is 10.00-20.00 mol%; and / or, The molar percentage of B2O3 is 0.00 to 10.00 mol%.

7. The ion sieve for absorbing lithium ions according to claim 2, characterized in that: The molar percentage of SiO2 is 30.00-50.00 mol%; and / or, The molar percentage of Na2O is 45.00-65.00 mol%; and / or, The molar percentage of Al2O3 is 4.00-15.00 mol%; and / or, The molar percentage of B2O3 is 0.00 to 5.00 mol%.

8. The ion sieve for absorbing lithium ions according to any one of claims 1 to 7, characterized in that: Based on the mass of the molten salt bath, 1wt% of the ion sieve is added to a molten salt bath containing 800ppm-1000ppm of lithium ions. After reacting at 500°C for 12 hours, the absorption rate of the ion sieve for lithium ions is ≥55.00%, and / or, Based on the mass of the molten salt bath, 1wt% of the ion sieve is added to a molten salt bath containing 10ppm-200ppm of lithium ions. After reacting at 500°C for 12 hours, the absorption rate of the ion sieve for lithium ions is ≥75%, and / or, The ion sieve is placed in a 5wt% HCl aqueous solution and soaked at 95°C for 18 hours, and the weight loss percentage of the ion sieve is ≥28.00%.

9. The ion sieve for absorbing lithium ions according to claim 8, characterized in that: Based on the mass of the molten salt bath, 1wt% of the ion sieve is added to a molten salt bath containing 800ppm-1000ppm of lithium ions. After reacting at 500°C for 12 hours, the absorption rate of the ion sieve to lithium ions is ≥60.00%, and / or, Based on the mass of the molten salt bath, 1wt% of the ion sieve is added to a molten salt bath containing 10ppm-200ppm of lithium ions. After reacting at 500°C for 12 hours, the absorption rate of the ion sieve for lithium ions is ≥80%, and / or, The ion sieve is placed in a 5wt% HCl aqueous solution and soaked at 95°C for 18 hours, and the weight loss percentage of the ion sieve is ≥30.00%.

10. The ion sieve for absorbing lithium ions according to claim 8, characterized in that: The ion sieve is placed in a 5wt% HCl aqueous solution and soaked at 95°C for 18 hours, and the weight loss percentage of the ion sieve is ≥36.00%.

11. The ion sieve for absorbing lithium ions according to any one of claims 1 to 7, characterized in that: The ion sieve is in a granular, sheet or porous form.

12. The ion sieve for absorbing lithium ions according to claim 11, characterized in that: The particle size of the granular ion sieve is 1 mm-4 mm; and / or, The thickness of the sheet-like ion sieve is 0.3 mm-1.0 mm.

13. The ion sieve for absorbing lithium ions according to claim 8, characterized in that: The ion sieve is in a granular, sheet or porous form.

14. The method for preparing an ion sieve for absorbing lithium ions according to any one of claims 1 to 13, characterized in that: The ion sieve is prepared by preparing the ingredients according to any one of claims 1 to 13, and then melting, molding and cooling.

15. The preparation method according to claim 14, characterized in that: The temperature of the melting treatment is 1000°C to 1650°C.

16. Use of the ion sieve for absorbing lithium ions according to any one of claims 1 to 13 or the ion sieve for absorbing lithium ions obtained by the preparation method according to claim 14 or 15 in the field of recovering lithium from lithium-containing waste glass, recovering lithium from waste battery materials, or manufacturing chemically strengthened glass.

17. A method for recovering lithium from a molten salt bath for chemically strengthened glass production, characterized in that: The steps include: (1) adding the lithium-containing glass to be chemically strengthened and the ion sieve for absorbing lithium ions according to any one of claims 1 to 13 or the ion sieve for absorbing lithium ions obtained by the preparation method according to claim 14 or 15 together into a molten salt bath for chemical strengthening, or adding the ion sieve for absorbing lithium ions according to any one of claims 1 to 13 or the ion sieve for absorbing lithium ions obtained by the preparation method according to claim 14 or 15 into a molten salt bath containing lithium ions after chemical strengthening, and using the ion sieve to absorb the lithium ions released by the glass into the molten salt bath; (2) subjecting the ion sieve having absorbed lithium ions in step (1) to acid hydrolysis, and filtering to obtain an acid hydrolysis solution; (3) adding a first ion precipitant to the acid hydrolysis solution obtained in step (2) to precipitate impurity aluminum ions in the acid hydrolysis solution, filtering, adding a second ion precipitant to the obtained filtrate to precipitate lithium ions in the filtrate, filtering to obtain a reusable lithium-containing material.

18. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 17, wherein: The temperature of the molten salt bath is 310°C to 650°C; and / or, The added amount of the ion sieve is 0.1-20.0 wt % based on the mass of the molten salt bath for chemical strengthening.

19. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 18, wherein: The temperature of the molten salt bath is 380°C to 650°C.

20. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 18, wherein: The temperature of the molten salt bath is 400°C to 650°C.

21. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 18, wherein: The molten salt bath for chemical strengthening contains sodium ions.

22. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 18, wherein: The chemical strengthening molten salt bath contains 5wt% to 100wt% of a sodium salt, and the sodium salt includes at least one of sodium nitrate, sodium chloride and sodium sulfate.

23. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 22, wherein: The sodium salt is sodium nitrate.

24. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to any one of claims 17 to 23, characterized in that: In step (2), the acid solution for acid hydrolysis treatment includes aqueous hydrochloric acid solution and / or aqueous nitric acid solution; and / or, In step (3), the first ion precipitation agent is an alkaline solution; and / or, The second ion precipitation agent is a soluble carbonate.

25. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 24, wherein: In step (2), the concentration of the acid solution is greater than or equal to 5 wt %.

26. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 24, wherein: The temperature of the acid hydrolysis treatment is 25°C to 95°C.

27. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 26, wherein: The acid hydrolysis treatment time is 8~24h.

28. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 24, wherein: In step (3), the first ion precipitant is ammonia water.

29. The method for recovering lithium from a molten salt bath for producing chemically strengthened glass according to claim 24, wherein: In step (3), the second ion precipitant is sodium carbonate.

30. A method for producing chemically strengthened glass, characterized in that: The invention comprises the following steps: a process of adding the ion sieve for absorbing lithium ions described in any one of claims 1 to 13 or the ion sieve for absorbing lithium ions obtained by the preparation method described in claim 14 or 15 to a molten salt bath for chemical strengthening of glass, and a process of bringing the lithium-containing glass into contact with the molten salt bath to perform ion exchange.

31. The method for producing chemically strengthened glass according to claim 30, wherein: The temperature of the chemical strengthening molten salt bath is 310°C to 650°C; and / or, The added amount of the ion sieve is 0.1-20.0 wt % based on the mass of the molten salt bath for chemical strengthening.

32. The method for producing chemically strengthened glass according to claim 31, wherein: The temperature of the chemical strengthening molten salt bath is 380°C to 650°C.

33. The method for producing chemically strengthened glass according to claim 31, wherein: The temperature of the chemical strengthening molten salt bath is 400°C to 650°C.

34. The method for producing chemically strengthened glass according to claim 31, wherein: After the step of adding the ion sieve to the chemical strengthening molten salt bath, the Li ion concentration in the chemical strengthening molten salt bath is 500 ppm or less.

35. The method for producing chemically strengthened glass according to claim 31, wherein: The molten salt bath contains sodium ions; the molten salt bath is at least one of nitrate, sulfate and chloride.

36. The method for producing chemically strengthened glass according to claim 35, wherein: The molten salt bath is nitrate.

37. The method for producing a chemically strengthened glass according to any one of claims 30 to 36, wherein: The method for producing chemically strengthened glass further includes a step of recovering lithium from the ion sieve added to the molten salt bath and used by an acid hydrolysis treatment process and a separation treatment process.