Induction low temperature brazing solder paste, sealing method and device
Through induction low-temperature brazing technology and the use of brazing paste, the problems of welding deformation of stainless steel sheets and short sealant life are solved, and efficient and environmentally friendly welding sealing effect is achieved, which enhances the welding quality and service life.
Patent Information
- Application Number
- CN202410427214.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-10
AI Technical Summary
Stainless steel sheets are prone to deformation and burning through during welding, and the existing sealant has a short service life and is not environmentally friendly, resulting in insufficient airtightness and connection stability of the welds.
The brazing paste and sealing method for induction low-temperature brazing are composed of flux and metal powder with specific ratios. They are melted and solidified by induction heating to fill the gaps, combined with a three-dimensional visual recognition system and real-time temperature measurement. The system and laser ranging and deviation correction system carry out precise control to ensure low-temperature welding and efficient sealing.
Improves welding quality and sealing, extends service life, reduces the probability of thermal deformation, and uses tin-based filling materials and large-grain copper powder to form a copper skeleton structure, enhancing gap strength and welding reliability, ensuring environmental protection and high efficiency Welding process.
Smart Images

Figure CN118081175B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of welding technology, and in particular to an induction low-temperature brazing sealing method, brazing material and device. Background Art
[0002] At present, the materials used for rail vehicle bodies are mainly divided into three types: ordinary steel, stainless steel and aluminum alloy. Stainless steel as a body material has excellent properties such as high strength, high temperature resistance and corrosion resistance, and has become a new research hotspot. With the demand for body weight reduction, 0.6mm-1mm stainless steel sheets are becoming more and more widely used. For thin plates, melting welding is prone to deformation and burn-through defects, and subsequent repairs are very difficult. The stainless steel body connection process usually adopts resistance spot welding, and the overlap gap needs to be sealed at the same time. However, with the increase in the speed level of stainless steel vehicles, the demand for airtight stability and long-term connection performance of the body weld is becoming increasingly urgent. At present, the main method used is to apply sealant, which is not environmentally friendly and easy to age and fall off; therefore, an induction low-temperature brazing solder paste, sealing method and device are proposed to solve the problems of easy aging, short service life and poor sealing of the overlap gap sealant mentioned above. Summary of the invention
[0003] One of the purposes of the present application is to provide a solder paste for induction low temperature brazing.
[0004] Another object of the present application is to provide an induction low-temperature brazing sealing method.
[0005] To achieve the above objectives, the technical solution adopted in the present application is: a solder paste for induction low-temperature brazing, wherein the solder paste comprises 11-13% flux and 87-89% metal powder in percentage by mass; the flux raw materials comprise 30-40% rosin, 3-5% thixotropic agent, 10-15% activator, 3-5% surfactant, 30-40% solvent, and 3-5% corrosion inhibitor in percentage by mass; the metal powder raw materials comprise 85-92% alloy powder and 8-15% filling medium in percentage by mass; the alloy powder comprises one or two of Sn0.5Cu, Sn3Ag0.5Cu, and Sn0.3Ag0.7Cu; the filling medium is copper powder, the particle size of the copper powder is larger than that of the alloy powder, the particle size of the alloy powder is 10-25um, and the particle size of the copper powder is 40-60um.
[0006] An induction low-temperature brazing sealing method comprises the following steps:
[0007] S100: preparing the solder paste for induction low temperature brazing as described above;
[0008] S200: pre-processing the two workpieces, and then overlapping the two workpieces;
[0009] S300: Fill the solder paste into the overlapping junction of the two workpieces;
[0010] S400: induction heating the solder paste until it melts, so that the melted liquid solder paste spreads and fills the overlap gap between the two workpieces; the induction heating temperature is between 300°C and 450°C;
[0011] S500: Cooling to room temperature to solidify the solder paste and seal the gap;
[0012] S600: Post-processing the sealed workpiece.
[0013] Compared with the prior art, the beneficial effects of this application are:
[0014] (1) The present invention provides a flux containing a specific ratio. The interaction between the components can make the performance of the flux better, thereby improving the brazing quality and efficiency, and making the sealing of the workpiece after brazing smoother and more reliable, thereby greatly improving the service life of the overlap seal of the workpiece.
[0015] (2) The filling material is tin-based, which has a low melting point, and can perform low-temperature sealing welding on the workpiece, reducing the probability of thermal deformation of the workpiece. At the same time, the filling material does not contain lead elements and is environmentally friendly and pollution-free. On the other hand, large-particle copper powder is used. The copper particles react with Sn during the packaging process to generate Cu6Sn5 reinforcement phase, which will accumulate at the entrance of the lap joint to form a copper skeleton structure, which can effectively seal the gap between the two plates, thereby ensuring welding quality and reliability and enhancing gap strength.
[0016] (3) Induction heating is adopted, which belongs to indirect heating. The heating module of the device adopts high-frequency induction heating method of indirect contact heating, and the flat applicable coil is designed to effectively control the heat input and heat distribution, so as to ensure the heat distribution of relatively direct heating of thick plates and relatively indirect heating of thin plates during the brazing process, thereby ensuring the low temperature of the whole brazing process, especially the low temperature of thin plates, and ensuring the small deformation of thin plates. At the same time, a preheating coil is also provided, which preheats the brazing paste on the one hand and preheats the workpiece to be processed on the other hand, so as to more easily achieve and ensure the low temperature of the whole brazing process.
[0017] (4) The device's three-dimensional visual recognition system can analyze the assembly gap in real time and adaptively adjust the amount of solder paste added; the device's real-time temperature measurement system can detect the temperature in real time to ensure that the heated parts of the metal can be controlled below the set temperature during the entire brazing process; the device's laser ranging and correction system can detect the distance in real time and implement feedback correction to ensure the position control and process stability of the entire brazing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the overall structure of the present invention.
[0019] Figure 2 It is a schematic structural diagram of two workpieces during sealing welding of the present invention.
[0020] Figure 3 It is a schematic diagram of the heating coil structure of the present invention.
[0021] Figure 4 It is a schematic diagram of the filling and melting sealing process of the solder paste of the present invention.
[0022] Figure 5 It is a schematic diagram of the copper skeleton structure formed by the accumulation of Cu6Sn5 reinforcement phase in the solder paste of the present invention.
[0023] In the figure: 1. workbench; 2. moving mechanism; 3. feeding module; 4. induction heating module; 401. main heating coil; 5. image recognition module. DETAILED DESCRIPTION
[0024] Below, the present application is further described in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.
[0025] In the description of the present application, it should be noted that directional words, such as the terms "center", "lateral", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc., indicating directions and positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of narrating the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and cannot be understood as limiting the specific scope of protection of the present application.
[0026] It should be noted that the terms "first", "second", etc. in the description and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.
[0027] One of the preferred embodiments of the present application is as follows: Figures 1 to 5 As shown, a solder paste for induction low temperature brazing comprises, by weight percentage, 11-13% of flux and 87-89% of metal powder.
[0028] Specifically, the preparation method of the solder paste is as follows: a certain amount of soldering flux and metal powder are weighed respectively according to the formula ratio, and the two are poured into a blender, and the solder paste can be obtained by stirring and mixing.
[0029] like Figure 4 As shown, when in use, fill the solder paste between the two overlapping workpieces, then heat it to melt the solder paste, and the melted liquid solder paste will flow into the gap between the two workpieces, and then wait for the liquid solder paste to condense into a solid weld. Compared with the original use of sealant to fill the gap between the two workpieces, the present application uses the solder paste to heat, melt and solidify to fill the gap, that is, to achieve high-reliability sealing performance through metallurgical bonding, strong bonding force, high dynamic fatigue performance, and can effectively improve the joint strength and durability of the workpiece. This method is not only easy to operate, but also can avoid the problem of deformation or aging of the original sealant in high temperature or high humidity environment, thereby ensuring the long-term stability and reliability of the workpiece. Through the use of solder paste, a sealed connection between workpieces can be achieved, ensuring that the product has good performance and service life under various environmental conditions.
[0030] It can be understood that, in terms of mass percentage, the flux raw materials include: 30-40% rosin, 3-5% thixotropic agent, 10-15% activator, 3-5% surfactant, 30-40% solvent, and 3-5% corrosion inhibitor.
[0031] As a further description of the above embodiment: flux is an indispensable auxiliary material in brazing. It has the function of removing oxides on the surface of the object to be soldered (workpiece) and reducing the surface finishing of the solder. It has a great influence on the quality of welding. There are many types of flux. There are two main uses of flux. One is to use it alone during wave soldering, and the other is to use it mixed with solder during reflow soldering. Although the usage is different, the role they play is the same. There are many components of rosin, thixotropic agent, activator, surfactant, solvent and corrosion inhibitor in the flux. The specific components are provided below for reference:
[0032] (1) Rosin: one or more of polymerized rosin, ice white rosin and AX-E rosin.
[0033] The main function of rosin in flux is to remove surface oxides on the workpiece. Rosin is corrosive. Heating and melting it can corrode the surface oxide film of the workpiece. At the same time, the melted rosin will float on the surface of the solder. After cooling, it will form an isolation layer on the welding surface to prevent the welding surface from being oxidized again. In addition, rosin can also increase the fluidity of the solder, which helps to increase wettability, and also make the solder joints fuller and reduce the occurrence of cold solder joints.
[0034] (2) Thixotropic agent: castor oil type, polyamide type thixotropic agent, one or both of them.
[0035] This component is mainly used to adjust the viscosity and printing performance of the solder paste to prevent the solder paste from tailing, sticking, etc. after extrusion or printing.
[0036] (3) Surfactant: one or more of succinic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, and phenylsuccinic acid.
[0037] This component is used as flux acid in solder paste, and has good fluxing and acidifying activity, which can effectively improve the quality and efficiency of welding. In addition, this component can also reduce the oxides generated during welding, reduce the possibility of pores and cracks in the welding process, thereby improving the reliability and stability of the product. Therefore, adding this component to solder paste can significantly improve the welding effect and make the welding process smoother and more reliable.
[0038] (4) Surfactant: one or more of 2, 3-dibromosuccinic acid, amines, aniline, and triethanolamine.
[0039] It should be known that during the soldering process, the solder paste will be in a liquid state after being heated and melted, while the workpiece is in a fixed state. When the liquid solder paste contacts the solid workpiece, the tension is quite large. If the surface tension of the liquid solder paste cannot be effectively reduced, when the liquid solder paste is converted into a solid solder joint, the shape should be spherical, and it does not have a suitable wetting angle. At the same time, it cannot cover the gap between the two workpieces or cannot spread and infiltrate the required welding and sealing parts. The main function of the surfactant in the flux is to reduce the surface tension of the flux and increase the affinity of the flux to the nail material and the welded parts, so that the flux can completely cover the solder and the welded workpiece, so that the flux can fully remove the oxide film and oil stains on the surface of the welded base material, prevent the solder joint from being oxidized after welding, and ensure the quality and reliability of the solder joint.
[0040] Therefore, by adding surfactants with relatively large polarity, the flux molecules have greater polarity to reduce the surface tension of the flux, promote the van der Waals force or chemical force between the flux and the solder and the surface to be soldered to improve the wetting properties of the flux and make the solder and the welded parts in good contact.
[0041] (5) Solvents: one or more of the following: ethanol, tetrahydrofurfuryl alcohol and terpineol from the monohydric alcohol class; ethylene glycol, dipropylene glycol, tripropylene glycol and 1,2-propylene glycol from the dihydric alcohol class; propylene glycol methyl ether, dipropylene glycol methyl ether, tetraethylene glycol dimethyl ether and diethylene glycol from the ether class.
[0042] Solvent is an important component of flux. The solvent in the flux must not only provide good protection for the welding surface, but also have appropriate viscosity. Generally, organic solvents are used.
[0043] (6) Corrosion inhibitor: one or more of benzotriazole, quinoline, and methylbenzotriazole.
[0044] Corrosion inhibitor It is a highly effective corrosion inhibitor for copper. Its addition can inhibit the corrosion of copper plates caused by the active agent in the flux. It is generally believed that benzotriazole reacts with copper to form a precipitation film of insoluble polymer.
[0045] In summary, the interaction between the components of the flux, which is a combination of multiple ingredients, can make the performance of the flux better, thereby improving the welding quality and efficiency. Through this ratio of flux, it can play a role in cleaning the surface and improving wettability during the welding process, making the sealing of the workpiece after welding smoother and more reliable.
[0046] In one embodiment of the present application, the alloy powder includes one or two of Sn0.5Cu, Sn3Ag0.5Cu, and Sn0.3Ag0.7Cu.
[0047] It is understandable that the traditional flux alloy powder contains lead, while the filling material in this application is tin-based, which has a low melting point, below 300 degrees Celsius, and is easy to melt at "low temperature"; on the other hand, since it does not contain lead, it is environmentally friendly and pollution-free, and can better meet the needs of modern society for green and environmentally friendly materials. By using tin-based filling materials, not only can the safety and quality of the product be ensured, but the impact on the environment can also be reduced, reflecting the company's sense of responsibility for sustainable development.
[0048] Furthermore, the filling medium can be copper powder, that is, copper powder can be added to the solder paste. It is understandable that during the soldering process, the copper powder is wetted and flowed by the tin alloy and accumulated at the entrance of the overlap gap. The copper powder strengthens the rigidity of the solder and improves the thermal cycle fatigue resistance. In addition, the Cu particles react with Sn during the packaging process to generate a Cu6Sn5 reinforcement phase. During the solidification process, Cu6Sn5 is first precipitated. The solder joint strengthening effect comes from the mixed phase structure presented by Cu6Sn5 in the solder paste, such as Figure 5As shown in the figure, this mixed phase structure can improve the strength and stability of the brazing seam, that is, the Cu6Sn5 reinforcement phase is accumulated to form a copper skeleton structure, which can then well seal the gap between the two plates, thereby ensuring the quality and reliability of brazing, enhancing the gap strength, increasing its creep resistance, and improving the bonding strength, thereby improving the reliability and durability of the welding joint. In addition, copper powder can also effectively improve the thermal conductivity of the welding point, reduce heat concentration, and avoid welding quality problems caused by excessive temperature of the welding point. Therefore, adding copper powder in the welding process can effectively improve the performance of the welding joint and improve the welding quality and reliability.
[0049] More advanced, the particle size of the copper powder is preferably larger than the particle size of the alloy powder. It is understandable that the conventional copper powder particle size is about 10-25um, while the copper powder particle size here can be between 40-60um. It should be known that the particle size of large particles can improve the strength of the entire weld skeleton after brazing, because larger particles can provide better mechanical support, making the weld stronger; in addition, large-particle copper powder can also improve the electrical conductivity and thermal conductivity of the welding area, making the welding effect more stable and reliable, and ensuring the welding quality. Therefore, when selecting copper powder, pay attention to the optimization of particle size to ensure the stability and reliability of the final welding effect. By reasonably selecting copper powder with a larger particle size, the strength and stability of the weld can be effectively improved, thereby improving the welding quality and efficiency.
[0050] Another aspect of the present application also provides an induction low-temperature brazing sealing method, comprising the following steps:
[0051] S100: preparing the solder paste for induction low temperature brazing as described above.
[0052] S200: Pre-processing the two workpieces, and then overlapping the two workpieces.
[0053] S300: Fill the solder paste into the overlapping junction of the two workpieces.
[0054] S400: Induction heating the solder paste until it melts, so that the melted liquid solder paste spreads and fills the overlapping gap between the two workpieces; S500: Cooling to room temperature, so that the solder paste solidifies and seals the gap.
[0055] S600: Post-processing the sealed workpiece.
[0056] As a further description of the above steps:
[0057] In step S200, there are many ways of pretreatment, and this application only provides one specific implementation method for reference: it includes grinding, cleaning and drying the workpiece. It is understandable that before welding and sealing, the surface of the workpiece may have oil stains or oxide films, and then the oil stains or oxide films are removed by grinding, and then the dust generated on the surface of the workpiece after grinding is washed, and finally the washed workpiece is dried, so as to prepare for the subsequent welding and sealing, and improve the quality of the welding and sealing.
[0058] In step S400, induction heating is used. It should be noted that the melting temperature of the above-mentioned solder paste is about 220°C, and the workpiece to be welded and sealed may be thin. The welding temperature should be controlled below 450°C. Therefore, in order to ensure sufficient melting of the solder paste and reduce the impact of high temperature on the workpiece, "low temperature" welding can be used, that is, the induction heating temperature is preferably between 300°C and 450°C, and the specific temperature should be adjusted according to the actual situation and the characteristics of the workpiece to ensure the welding quality and the safety of the workpiece.
[0059] In step S600, after the welding condenses, the welds of the two workpieces may be uneven, which may affect the subsequent processing steps or aesthetics. Therefore, post-processing includes grinding the welds of the workpieces; that is, grinding the sealed welds by grinding equipment. Of course, grinding equipment is also common knowledge known to technicians in this field.
[0060] Another aspect of the present application also provides an induction low-temperature brazing device for implementing the above-mentioned induction low-temperature brazing sealing method, such as Figure 1-4 As shown, it includes a workbench 1, a moving mechanism 2, a feeding module 3, an induction heating module 4 and an image recognition module 5. The workbench 1 has a placement area for placing workpieces, the moving mechanism 2 is installed on the workbench 1, the feeding module 3 is installed on the moving mechanism 2, the induction heating module 4 is installed on the moving mechanism 2, and the image recognition module 5 is installed on the moving mechanism 2 and is electrically connected to the feeding module 3 and the induction heating module 4.
[0061] It can be understood that when performing sealing welding, the image recognition module 5 can identify the overlapping joints of the two workpieces, and then the feeding module 3 and the induction heating module 4 can perform the first process and the second process under the drive of the image recognition module 5, wherein the first process: the feeding module 3 can fill the solder paste into the overlapping joints of the two workpieces; the second process: the induction heating module 4 can heat and melt the solder paste.
[0062] Furthermore, the image recognition module 5 includes a three-dimensional visual recognition system, which can analyze the assembly gap of the workpiece in real time, and then the feeding module 3 can accurately fill the solder paste under the drive of the three-dimensional visual recognition system. It can be understood that the three-dimensional visual recognition system of the device can analyze the assembly gap of the workpiece in real time, and then the feeding module 3 can also adjust the amount of solder paste added according to the size of the gap to ensure that the welding effect of each workpiece reaches the best state.
[0063] It should be known that the induction heating module 4 generally includes a main heating coil 401, and the existing heating rings are generally "coil" or "spiral" structures, and the weld is a long and narrow structure. Although it can heat and melt the solder paste at the weld, due to its large heating range, it may cause certain thermal deformation to the thin plate, thereby affecting the quality and service life of the workpiece; and on the other hand, the area that does not need to be heated will also cause heat waste when the heating ring is working, so that its heat cannot be fully utilized, thereby affecting the efficiency of welding and the waste of energy.
[0064] In order to solve the above technical problems, in one embodiment of the present application, a heating zone parallel to the weld of the workpiece is provided at the bottom end of the main heating coil 401. Figure 3 As shown, two specific structures are provided for reference: Structure 1, the main heating coil 401 is a triangular structure as a whole; Structure 2, the main heating coil 401 is a "D" shaped structure as a whole. Regardless of which structure is adopted, the bottom end must be a "long strip" structure. In this way, when the solder paste is heated, it can fully heat the solder paste, and the heat transferred to the workpiece can be greatly reduced, so that the workpiece is in a low temperature state, which can greatly reduce the probability of deformation of the workpiece (especially thin plates).
[0065] Of course, the induction heating module 4 also includes a preheating coil, such as Figure 2As shown, the preheating coil is installed at the feeding port of the feeding module 3; it is understandable that the heating temperature of the preheating coil is definitely lower than the heating temperature of the main heating coil 401; that is, when the solder paste is extruded, the preheating coil can initially heat the extruded solder paste and the overlapping gap of the lower plate, but the heating temperature will not melt the solder paste, so that when the subsequent main heating coil 401 heats the solder paste at the gap, the solder paste itself has an initial temperature, and the melting rate of the solder paste will also increase, thereby improving the efficiency and quality of brazing. The setting of the preheating coil can not only speed up the melting speed of the solder paste, but also avoid damage to the plate caused by excessive temperature, thereby achieving low-temperature brazing, thereby better protecting the workpiece. By reasonably setting the temperature and heating time of the preheating coil and the main heating coil 401, a more accurate and efficient brazing operation can be achieved.
[0066] Finally, it should be noted that the moving mechanism 2 (three-dimensional movement of X, Y, and Z), the feeding module 3, the induction heating module 4, and the image recognition module 5 are all common knowledge known to those skilled in the art, and the control method is automatically controlled by a controller. The control circuit of the controller can be implemented by simple programming by technicians in this field, which is also common knowledge in this field. Therefore, this application document will no longer explain the control method and circuit connection in detail.
[0067] The working principle and method of the present invention are:
[0068] S100: First, prepare the solder paste, that is, weigh and mix the flux and metal powder according to the formula ratio to obtain the solder paste, and then add the solder paste into the feeding module 3.
[0069] S200: Clean the surfaces of the two workpieces, such as Figure 1 As shown, the cleaned workpiece is then placed on the placement area of the workbench 1 so that the two workpieces are overlapped; here we take a thin plate on a rail vehicle body overlapped on a thick plate as an example for explanation.
[0070] S300: Under the action of the moving mechanism 2 and the image recognition module 5, the feeding module 3 can accurately fill the solder paste at the junction (gap) of the two workpieces; Figure 4 As shown in (a) in .
[0071] S400: Under the action of the moving mechanism 2 and the image recognition module 5, the induction heating module 4 induction heats the solder paste until it melts; Figure 4 As shown in (b) in the figure. Then the melted liquid solder paste will spread and fill the overlap gap between the two workpieces; Figure 4 As shown in (c) in .
[0072] Of course, a real-time temperature measurement system can also be set up during this process to ensure that the heated metal parts can be controlled below 450°C during the entire brazing process; a laser ranging and correction system can also be set up, which can detect the distance in real time and implement feedback correction to ensure the position control and process stability of the entire brazing process.
[0073] On the other hand, step S300 and step S400 can also be performed simultaneously, that is, the addition of solder paste and induction heating are performed simultaneously, and the device can achieve efficient brazing and improve production efficiency. This synchronous operation can ensure that the solder paste is fully melted and evenly coated on the surface of the workpiece, and at the same time, the induction heating can quickly heat the workpiece to the brazing temperature, reduce the brazing time, and increase the speed of welding and sealing.
[0074] S500: Cooling to room temperature to solidify the solder paste and seal the gap.
[0075] S600: Post-process the sealed workpiece, that is, polish and beautify the solidified weld.
[0076] The above describes the basic principles, main features and advantages of the present application. Those skilled in the art should understand that the present application is not limited by the above embodiments, and the above embodiments and the specification only describe the principles of the present application. The present application may have various changes and improvements without departing from the spirit and scope of the present application, and these changes and improvements fall within the scope of the present application for which protection is sought. The scope of protection claimed by the present application is defined by the attached claims and their equivalents.
Claims
1. A solder paste for induction low temperature brazing, characterized in that: In terms of mass percentage, the solder paste includes 11-13% flux and 87-89% metal powder; in terms of mass percentage, the flux raw materials include: 30-40% rosin, 3-5% thixotropic agent, 10-15% activator, 3-5% surfactant, 30-40% solvent, and 3-5% corrosion inhibitor; in terms of mass percentage, the metal powder raw materials include 85-92% alloy powder and 8-15% filling medium; the alloy powder includes one or two of Sn0.5Cu, Sn3Ag0.5Cu, and Sn0.3Ag0.7Cu; the filling medium is copper powder, the particle size of the copper powder is larger than that of the alloy powder, the particle size of the alloy powder is 10-25um, and the particle size of the copper powder is 40-60um.
2. An induction low temperature brazing sealing method, characterized in that: The steps include: S100: preparing the solder paste for induction low temperature brazing as claimed in claim 1; S200: pre-processing the two workpieces, and then overlapping the two workpieces; S300: Fill the solder paste into the overlapping junction of the two workpieces; S400: induction heating the solder paste until it melts, so that the melted liquid solder paste spreads and fills the overlap gap between the two workpieces; the induction heating temperature is between 300°C and 450°C; S5 00: Cooling to room temperature to solidify the solder paste and seal the gap; S600: Post-processing the sealed workpiece.