A method for preparing a high-capacity leaching resin with surface-bonded polycationic phosphonate
The surface bonded polycationic phosphonate high-capacity extraction resin was prepared by suspension polymerization, which solved the defects of existing organic phosphonate extracting agents, achieved the function of efficient extraction of rare earths and precious metal ions, and improved the extraction stability and capacity.
Patent Information
- Application Number
- CN202410272536.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-03-11
AI Technical Summary
The existing organic phosphonate extractant has defects such as volatile, easy loss, emulsification of the third phase, flammability, and toxicity in rare earth hydrometallurgy. The extraction capacity of the bonded extractive resin is small, which limits its application value. .
The high-capacity extraction resin with surface bonded polycationic phosphonate was prepared by suspended polymerization, and the extraction capacity was improved by graft-from graft polymerization.
It achieves extraction performance with high capacity, rapid miscible in metal brine solution and deep diffusion, improves extraction stability and functional diversity, and is suitable for the extraction and separation of precious metals and rare earth ions.
Smart Images

Figure CN118085199B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-capacity leaching resin with surface-bonded polycationic phosphonate, in particular to a high-capacity polystyrene-based leaching resin with surface-bonded polyquaternary ammonium cationic phosphonate, belonging to the field of functional polymer materials. Technical Background
[0002] Professionals know that the separation of rare earth elements is the key to the development of the rare earth metallurgical industry. Small molecule organic phosphoric acid and its esters, or organic phosphonic acid and its esters have strong affinity and high coordination ability for rare earth ions. They are the most widely used solvent extractants in the rare earth hydrometallurgical industry, with many varieties and excellent performance. However, the selectivity, loading capacity, stripping efficiency, water dispersibility, emulsification phenomenon, extraction chemical stability, recycling and regeneration, and process loss of small molecule organic phosphonates as solution extractants determine their industrial use value for extracting and separating rare earths. In order to solve the defects of traditional organic phosphonate extractants such as volatility, easy loss, emulsified third phase, flammability, and toxicity, scientists have immobilized organic phosphonates on the surface of macroporous polystyrene, silica gel and other materials by covalent bonding to form bonded leaching resins with the function of extracting rare earth ions from solutions. They have demonstrated high selectivity leaching performance in the fields of rare earth hydrometallurgy, enrichment and extraction and separation of precious metal ions in dilute solutions, simple and efficient solid-liquid separation, no loss in the process, and clean environment.
[0003] There are usually several methods for the immobilization of organic phosphonates: ①Use unsaturated phosphonates as phosphine-containing functional monomers to homopolymerize or copolymerize with other monomers to prepare polyphosphonate-containing polymer materials. Unsaturated phosphonate monomers mainly include vinyl phosphonates or allyl phosphonates. Such organic phosphonate monomers have a single function and few varieties; and phosphonates derived from acrylates or acrylamides as polymerizable monomers are also the research objects of phosphine-containing functional monomers at present, but such phosphine-containing functional monomers have relatively low chemical stability for extraction and high prices, which are therefore limited in practical applications. ②Amino, acetyl, epoxy, etc. are grafted onto the surface of materials such as polystyrene and silica gel, and then organic phosphonate extractants are bonded using Mannich reactions, phosphonylation reactions, substitution reactions, etc. However, due to the influence of the surface area of the material itself and the number of surface active functional groups, the number of amino, acetyl, and epoxy grafts is small, so the number of immobilization points for bonded organic phosphonate extractants is small, which limits the improvement space of its saturated adsorption capacity and extraction capacity. Therefore, the organic phosphonate bonded leaching resin prepared in this way has the disadvantage of small extraction capacity. ③ Use organic phosphine monomers to graft polymerize on the surface of polymer materials to achieve the phosphine function of polymer materials. The methods are diverse, the profiles are variable, and the performance and extraction capacity are adjustable. However, this method has an insurmountable defect, which is the homopolymerization problem of organic phosphine monomer raw materials during the graft polymerization process, which not only causes the ineffective consumption of organic phosphine monomer raw materials, but also brings a necessary cleaning process to the re-functionalization process after grafting on the surface of polymer materials. Summary of the invention
[0004] In order to overcome the defects of the prior art, the present invention provides a high-capacity leaching resin with surface-bonded polycationic phosphonate in combination with the structural characteristics of organic phosphine extractants and the technical requirements and application scope of polystyrene-based leaching resins, which is prepared by a suspension polymerization method using polystyrene-based resins with surface-bonded unsaturated cationic phosphonate and di-unsaturated cationic phosphonate as monomer raw materials;
[0005] The polystyrene-based resin with unsaturated cationic phosphonate bonded to the surface has a schematic structure of general formula (I) or general formula (II):
[0006]
[0007] The diunsaturated cationic phosphonate has a structure shown in the general formula (III) or the general formula (IV):
[0008]
[0009] Wherein the general formula (I), general formula (II), general formula (III) or general formula (IV) Refers to polystyrene-based resin, R1 and R2 are selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C18 Hydrocarbon or C1~C 18 Hydroxyl, X - Select Cl - Br - or I - One of Refers to C1~C 18 Alkylene or Where n is a natural number between 0 and 2000.
[0010] The polystyrene-based resin refers to a cross-linked or non-cross-linked polystyrene resin, or a cross-linked or non-cross-linked (olefin monomer-styrene) copolymer resin, the olefin monomer refers to one or more of vinyl chloride, vinyl acetate, methyl acrylate, ethyl acrylate, butyl acrylate, butadiene or acrylonitrile, and n is a natural number between 1 and 2000.
[0011] The specific preparation method of the high-capacity leaching resin with surface-bound polycationic phosphonate is as follows: weigh the surface-bound unsaturated cationic phosphonate and A diunsaturated cationic phosphonate and an aqueous initiator are mixed together in deionized water, stirred and dispersed uniformly, stirred and swelled at room temperature for 2 to 24 hours under N2 protection, poured into an organic solvent, stirred and dispersed for 0.5 to 2 hours, placed in a polymerization kettle, the material temperature in the polymerization kettle is increased to 50 to 90°C, stirred for reverse suspension polymerization reaction for 2 to 20 hours, the material temperature in the reaction kettle is lowered to room temperature, filtered, washed and dried to obtain a high-capacity leaching resin of a surface-bound polycationic phosphonate having a structure schematically shown in the general formula (I) or the general formula (II).
[0012] The amount of the organic solvent is 300-3000% of the mass of the surface-bound unsaturated cationic polystyrene-based resin, the amount of deionized water is 50-500% of the mass of the di-saturated cationic phosphonate, and the amount of the di-unsaturated cationic phosphonate is 100% of the mass of the surface-bound unsaturated cationic phosphonate. The amount of the aqueous initiator is 10 to 1000% of the mass of the diunsaturated cationic phosphonate. The amount of the aqueous initiator is 1.5 to 15% of the mass of the diunsaturated cationic phosphonate.
[0013] The surface-bound unsaturated cationic phosphonate The schematic structure of general formula (I) or general formula (II) is:
[0014]
[0015] The diunsaturated cationic phosphonate has a structure shown in the general formula (III) or the general formula (IV):
[0016]
[0017] Wherein the general formula (I), general formula (II), general formula (III) or general formula (IV) Refers to polystyrene-based resin, R1 and R2 are selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Hydroxyl, X - Select Cl - Br - or I - One of Refers to C1~C 18 Alkylene or Where n is a natural number between 0 and 2000.
[0018] The polystyrene-based resin refers to a cross-linked or non-cross-linked polystyrene resin, or a cross-linked or non-cross-linked (olefin monomer-styrene) copolymer resin, and the olefin monomer refers to one or more of vinyl chloride, vinyl acetate, methyl acrylate, ethyl acrylate, butyl acrylate, butadiene or acrylonitrile.
[0019] The aqueous initiator refers to one of azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, azobisisopropylimidazoline hydrochloride, potassium persulfate or ammonium persulfate.
[0020] The organic solvent is selected from one or more of toluene, xylene, chlorobenzene, decahydronaphthalene, carbon tetrachloride, 1,2-dichloroethane or petroleum ether (boiling range 60-90° C.).
[0021] The monomer raw materials required for preparing the high-capacity leaching resin of the surface-bonded polycationic phosphonate of the present invention include: ① surface-bonded unsaturated cationic phosphonate It is a macromolecular monomer of the high-capacity leaching resin-supported phosphonate, and its surface is bonded with an unsaturated cationic phosphonate. ② The diunsaturated cationic phosphonate is a highly water-soluble cationic phosphonate monomer, and is also used as a crosslinking agent in graft copolymerization, which is crucial to improving the grafting efficiency.
[0022] The two monomer raw materials are derived from the same substance, namely 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate. To this end, the present invention further provides the surface-bound unsaturated cationic phosphonate Disclosed are diunsaturated cationic phosphonates and a specific preparation method of 2-hydroxy-3-(unsaturated tertiary amino)propylphosphonate.
[0023] The surface-bound unsaturated cationic phosphonate It has the schematic structure of general formula (I) or general formula (II):
[0024]
[0025] Wherein the general formula (I) and the general formula (II) Refers to a polystyrene-based resin, wherein the polystyrene-based resin refers to a cross-linked or non-cross-linked polystyrene resin, or a cross-linked or non-cross-linked (olefin monomer-styrene) copolymer resin; wherein the olefin monomer refers to one or more of vinyl chloride, vinyl acetate, methyl acrylate, ethyl acrylate, butyl acrylate, butadiene or acrylonitrile.
[0026] The surface-bound unsaturated cationic phosphonate The specific preparation method is as follows: weigh the solvent and chloromethyl In a reactor, swell at room temperature for 24 hours under N2 protection, then add 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate and a polymerization inhibitor, adjust the temperature of the material in the reactor to 25-45°C, stir and react for 6-16 hours, then increase the reaction temperature to 60-90°C, continue to stir and react for 6-36 hours, and then filter, wash and dry to obtain a surface-bound unsaturated cationic phosphonate of general formula (I) and general formula (II)
[0027] The amount of solvent used is chloromethylated The amount of the 2-hydroxy-3-(unsaturated tertiary amino)propylphosphonate is 200-2000% by mass. The molar amount of the chloromethyl contained is 80-110%, and the amount of the polymerization inhibitor used is 0.1-10% of the weight of 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate.
[0028] The solvent refers to one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, tetrahydrofuran, 1,4-dioxane, 2-methoxyethanol, 2-ethoxyethanol, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.
[0029] The diunsaturated cationic phosphonate has a structure shown in the general formula (III) or the general formula (IV):
[0030]
[0031] Wherein R1 and R2 in the general formula (III) or the general formula (IV) are selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Hydroxyl group, Refers to C1~C18 Alkylene or X - Select Cl - Br - or I - One of the following; where n is a natural number between 0 and 2000.
[0032] The specific preparation method of the di-unsaturated cationic phosphonate is as follows: weigh a solvent, 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate, a dialkylating agent and a polymerization inhibitor respectively in a reaction kettle, raise the temperature of the materials in the reaction kettle to 20-90° C. under N2 protection, stir and react for 6-12 hours, and then filter, wash and dry to obtain a di-unsaturated cationic phosphonate having a structure represented by general formula (III) or general formula (IV);
[0033] The amount of the solvent is 50-200% of the total mass of the dialkylating agent and 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate, the molar ratio of the dialkylating agent to 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate is 0.48-0.55:1, and the amount of the inhibitor is 0.1-10% of the mass of 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate.
[0034] The dialkylating agent has a structure shown in general formula (VII):
[0035]
[0036] Wherein the general formula (VII) Select C1~C 18 Alkylene or Wherein n is a natural number between 0 and 2000, and X is one of Cl, Br or I.
[0037] The solvent refers to one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, tetrahydrofuran, 1,4-dioxane, 2-methoxyethanol, 2-ethoxyethanol, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide;
[0038] The unsaturated cationic phosphonate is bonded to the surface In the preparation methods of the resin and the di-unsaturated cationic phosphonate, a polymerization inhibitor is used, and the polymerization inhibitor refers to one or more of hydroquinone, p-methoxyphenol, tert-butylhydroquinone, 2,6-dibutylhydroquinone, 2,6-di-tert-butyl-p-cresol or 2,4,6-tri-tert-butylphenol.
[0039] An unsaturated cationic phosphonate is bonded to the surface In the preparation methods of the resin and the di-unsaturated cationic phosphonate, 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate is used. The 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate has a structure shown in the general formula (V) or the general formula (VI):
[0040]
[0041] Wherein R1 in the general formula (V) or the general formula (VI) is selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Hydroxyl group.
[0042] The 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate is prepared by the following method: weighing a phosphite ester and putting it into a reaction kettle, adding sodium alcoholate under N2 protection and stirring, raising the temperature of the material in the reaction kettle to 70-140°C, continuously adding N-glycidyl-N,N-diallylamine or N-glycidyl-N-alkyl-N-allylamine to the reaction kettle, stirring and reacting for 8-12 hours, separating and purifying to obtain 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonic acid dialkyl ester.
[0043] The amount of phosphite used is 200-2000% of the mass of N-glycidyl-N,N-diallylamine or N-glycidyl-N-alkyl-N-allylamine, and the amount of sodium alkoxide used is 0.5-5% of the mass of N-glycidyl-N,N-diallylamine or N-glycidyl-N-alkyl-N-allylamine.
[0044] The N-glycidyl-N-alkyl-N-allylamine has a structure shown in the general formula (VIII):
[0045]
[0046] The hydrocarbon group refers to R1 in the general formula (VIII), and R1 is selected from C1 to C 18 Hydrocarbon.
[0047] The phosphite has a structure shown in the general formula (IX):
[0048]
[0049] Wherein R2 in the general formula (IX) is selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Hydroxyl group.
[0050] The sodium alkoxide refers to one of sodium methoxide, sodium ethoxide, sodium propoxide or sodium butoxide.
[0051] The present invention provides a high-capacity leaching resin with surface-bonded polycationic phosphonate, which has the following beneficial effects:
[0052] ① The high-capacity leaching resin with a surface-bonded polycationic phosphonate provided by the present invention has not only phosphonate units bonded on its surface, but also the number of phosphonate units can be artificially controlled. At the same time, its surface has high hydrophilicity and can be quickly miscible in a metal salt aqueous solution, from which precious metal ions or rare earth ions can be quickly adsorbed and extracted.
[0053] ② After the high-capacity leaching resin with surface-bonded polycationic phosphonate provided by the present invention is fully swollen in an aqueous solution, the polycationic phosphonate layer grafted on its surface is expanded, and the pore size is close to the micron level or millimeter level, which is conducive to the in-depth diffusion of metal cations. Therefore, the ability of the polycationic phosphonate surface layer of the leaching resin to adsorb and extract metal cations can be fully demonstrated.
[0054] ③ The high-capacity leaching resin with surface-bound polycationic phosphonate provided by the present invention has multiple chemical activities, such as the hydrolysis or partial hydrolysis of the phosphonate unit, the oxidizability of the hydroxyl group, etc., thereby achieving the diversification of its functions and performances.
[0055] ④ The high-capacity leaching resin with surface-bonded polycationic phosphonate of the present invention requires only a few raw materials, all of which are industrial products, and the preparation method is simple and coordinated.
[0056] ⑤ The high-capacity leaching resin with surface-bonded polycationic phosphonate of the present invention has high extraction chemical stability and is particularly suitable for recycling in the process of extraction, separation or enrichment and recovery of precious metal ions or rare earth ions. DETAILED DESCRIPTION
[0057] The high-capacity leaching resin with surface-bound polycationic phosphonate and the preparation method thereof of the present invention are further described by the following examples, the purpose of which is to provide a better understanding of the content of the present invention.
[0058] Example 1 Preparation of high capacity leaching resin-1 with surface-bound polycationic phosphonate
[0059] Step 1: Preparation of diethyl 2-hydroxy-3-(N,N-diallylamino)propylphosphonate
[0060] Weigh 130 g of diethyl phosphite into a reactor, and slowly add 2.5 g of sodium ethoxide under N2 protection while stirring. Raise the temperature of the material in the reactor to 100-110°C, and slowly and continuously add 21 g of N-glycidyl-N,N-diallylamine to the reactor. After stirring for 8 hours, recover the excess diethyl phosphite by vacuum rotary evaporation, and then separate the residue to obtain 37.5 g of viscous light yellow liquid product. The product IR (cm-1 , KBr membrane) include: 3404 is the characteristic absorption peak of hydroxyl OH, 3029cm -1 is the characteristic absorption peak of vinyl CH, 2925, 2867 is the characteristic absorption peak of methyl and methylene, 1645 is the characteristic peak of C=C, 1479, 1428 are the characteristic absorption peaks of CN, 1257 is the characteristic absorption peak of P=O double bond, and 1042 is the characteristic absorption peak of POC; 1 H-NMR (CDCl3): 1.22 (t, 6H), 2.36 (m, 2H), 2.63 (m, 2H), 3.51 (m, 1H), 3.85 (d, 4H), 4.04 (m, 4H), 4.50 (m, 1H), 5.74 (m, 4H), 6.01 (m, 2H), it was determined that the product was 2-hydroxy-3-(N, N-diallylamino) propylphosphonic acid diethyl ester. Based on N-glycidyl-N, N-diallylamine, the yield of 2-hydroxy-3-(N, N-diallylamino) propylphosphonic acid diethyl ester was 93.7%. The following reaction formula-1 expresses the preparation process of 2-hydroxy-3-(N, N-diallylamino) propylphosphonic acid diethyl ester:
[0061]
[0062] Step 2: Surface bonding of unsaturated quaternary ammonium cation phosphonate Preparation of Resin-1
[0063] Weigh 60 grams of isobutyl alcohol, 60 grams of 1,4-dioxane, 10 grams of chlorine balls (cross-linking degree 10%, chlorine content 18.86%, particle size 0.23-0.45 mm purchased from Nankai University Chemical Plant), 16 grams of 2-hydroxy-3-(N,N-diallylamino)propylphosphonic acid diethyl ester and 0.08 grams of hydroquinone in a reactor, swell at room temperature for 24 hours under N2 protection, adjust the temperature of the materials in the reactor to 30-40°C, stir and react for 12 hours, then increase the temperature of the materials in the reactor to 70-80°C, continue to stir and react for 24 hours, filter, wash with ethanol and Soxhlet extraction for 24 hours, and vacuum dry to constant weight to obtain 23.6 grams of slightly yellow spherical product. This product was analyzed by elution titration for free Cl - The content is 7.08%, and the effective grafting rate is calculated to be about 85%; the characteristic peaks in the infrared spectrum of the product after the chlorine ball grafting include: FT-IR (cm -1 , KBr tablet): 3412cm -1 The characteristic absorption peak of hydroxyl group OH is 3031cm -1 Characteristic absorption peaks of vinyl, 2932, 2867cm -1 Characteristic absorption peaks of methyl and methylene, 1645 and 1478 cm-1 The characteristic absorption peak of benzene ring is 1256cm -1 Characteristic absorption peaks of P=O double bond, 1056, 1012 cm -1 The absorption peak of POC is shown at . The resin has been successfully grafted with quaternary ammonium cationic phosphonate. The following reaction equation-2 schematically expresses the surface-bonded unsaturated quaternary ammonium cationic phosphonate. Preparation process of resin-1:
[0064]
[0065] Step 3: Preparation of 1,4-bis(N,N-diallyl-N-(2-hydroxy-3-(diethoxyphosphonyl)propyl)ammonium)butane
[0066] Dissolve 13.7 g of 2-hydroxy-3-(N,N-diallylamino)propylphosphonic acid diethyl ester in 50 g of ethanol, add 5.5 g of 1,4-dibromobutane and 0.5 g of hydroquinone, and adjust the temperature of the reaction material liquid to 60-70°C under N2 protection. React for 18 hours, then lower the temperature of the reaction product system to room temperature. After standing, filter to obtain the crude product, purify it by recrystallization from ethanol, and vacuum dry it to constant weight to obtain 16.6 g of white crystalline product with a yield of about 87%. Chemical titration analysis of Br in the product - The content is 19.83%, which is consistent with the molecular formula C 30 H 60 The calculated Br content of Br2N2O8P2 is consistent with the theoretical value of 20.01%. Product spectrum analysis data: IR (cm -1 , KBr tablet): 3412cm -1 The characteristic absorption peaks of hydroxyl group OH are 2937 and 2868 cm -1 Characteristic absorption peaks of methyl and methylene, 1648 and 1437 cm -1 It is the characteristic absorption peak of CN, 1256cm -1 Characteristic absorption peaks of P=O double bond, 1138, 1016cm -1 It is the characteristic absorption peak of POC; 1H-NMR (δ, CD3OD): 1.31 (t, 4H), 1.73 (t, 4H), 2.18 (m, 2H), 3.24 (t, 8H), 3.29 (m, 4H), 3.52 (m, 4H), 3.82 (m, 2H), 3.92 (m, 8H), 4.04 (s, 4H), 4.16 (q, 4H), 4.52 (s, 4H), 4.90-5.11 (m, 12H). Based on the above analytical data, it was confirmed that the product was 1,4-bis(N,N-diallyl-N-(2-hydroxy-3-(diethoxyphosphonyl)propyl)ammonio)butane bromide. The following reaction formula-3 expresses the preparation process of 1,4-bis(bromide N,N-diallyl-N-(2-hydroxy-3-(diethylphosphinoyl)propyl)ammonium)butane:
[0067]
[0068] Step 4: High-capacity leaching resin-1 with surface-bonded polycationic phosphonate
[0069] Weigh 20.8 g of surface-bound unsaturated quaternary ammonium cation phosphonate Resin-1, 50 g of 1,4-bis(N,N-diallyl-N-(2-hydroxy-3-(diethoxyphosphonyl)propyl)ammonium)butane bromide and 1.65 g of azobisisobutylamidine hydrochloride were dissolved in 100 g of deionized water, stirred evenly, and poured into a reactor with 500 g of toluene. Stirred and dispersed for 1.5 hours under N2 protection, the temperature of the material in the reactor was raised to 50-55°C, and reverse suspension polymerization was performed for 2 hours. The temperature of the material in the reactor was raised to 70-80°C, and the polymerization reaction was continued for another 2 hours. The temperature of the material in the reactor was then lowered to room temperature, filtered, and washed with deionized water until there was no Cl in the washing water. - or Br - The product was dried and weighed to obtain 121.4 g of product, which was analyzed to be high capacity leaching resin-1 (referred to as HCER-1) with surface-bonded polycationic phosphonate, with a water content of about 41.7%. The grafting efficiency was calculated to be about 100%.
[0070] Example 2 Preparation of high capacity leaching resin-2 with surface-bound polycationic phosphonate
[0071] The method and steps of Example 1 were weighed, and the N-glycidyl-N,N-diallylamine in step 1 was replaced with N-glycidyl-N-benzyl-N-allylamine to obtain 2-hydroxy-3-(N-benzyl-N-allylamino)propylphosphonic acid diethyl ester; the 2-hydroxy-3-(N,N-diallylamino)propylphosphonic acid diethyl ester in step 2 was replaced with 2-hydroxy-3-(N-benzyl-N-diallylamino)propylphosphonic acid diethyl ester to obtain surface-bound unsaturated quaternary ammonium cationic phosphonate. Resin-2, see the following formula:
[0072]
[0073] The 1,4-dibromobutane in step 3 is replaced with 1,16-dibromohexadecane to obtain 1,16-bis(bromide N-allyl-N-benzyl-N-(2-hydroxy-3-(diethylphosphinoyl)propyl)ammonium)hexadecane.
[0074] Step 4: Weigh 20 grams of surface-bound unsaturated quaternary ammonium cationic phosphonate Resin-2, 80 g of 1,16-bis(bromide N-benzyl-N-allyl-N-(2-hydroxy-3-(diethylphosphinoyl)propyl)ammonium)hexadecane and 1.62 g of diisobutylazobenzamide hydrochloride were dissolved in 120 g of deionized water, stirred evenly, and poured into a reactor with 400 g of toluene. Stirred and dispersed for 1.5 hours under N2 protection, the temperature of the material in the reactor was raised to 50-55°C, and after 2 hours of polymerization, 0.62 g of diisobutylazobenzamide hydrochloride was added, the temperature of the material in the reactor was raised to 70-80°C, and the polymerization reaction was continued for 2 hours. Then, the temperature of the material in the reactor was lowered to room temperature, filtered, and washed with deionized water until there was no Cl in the washing water. - or Br - After drying, 157.4 g of product was obtained. Analysis showed that the product was high capacity leaching resin-2 (referred to as HCER-2) with surface-bonded polycationic phosphonate, with a water content of about 36.5%. The grafting efficiency was calculated to be about 100%.
[0075] Example 3 Preparation of high capacity leaching resin-3 with surface-bound polycationic phosphonate
[0076] According to the method and steps of Example 1, the 1,4-dibromobutane in step 3 is replaced with ɑ,ω-dibromopolyethylene glycol-200 (the chemical structure of ɑ,ω-dibromopolyethylene glycol-200 is Prepare α,ω-bis(bromide N,N-diallyl-N-(2-hydroxy-3-(diethylphosphinoyl)propyl)ammonium)polyethylene glycol-200, the chemical structure of which is shown in the following formula:
[0077]
[0078] Step 4: Weigh 20 grams of surface-bound unsaturated cationic phosphonate Resin-1, 165 g of α, ω-bis(bromide N, N-diallyl-N-(2-hydroxy-3-(diethylphosphinoyl)propyl)ammonium) polyethylene glycol-200 and 1.62 g of diisobutylamidine hydrochloride were dissolved in 400 g of deionized water, stirred evenly, and poured into a reactor with 1200 g of toluene. Stirred and dispersed for 1.5 hours under N2 protection, the temperature of the material in the reactor was raised to 50-55°C, and after 2 hours of polymerization, the temperature of the material in the reactor was raised to 70-80°C, and 0.65 g of diisobutylamidine hydrochloride was added twice before and after, and the polymerization reaction was continued for 2 hours. Then, the temperature of the material in the reactor was lowered to room temperature, filtered, and washed with deionized water until there was no Cl in the washing water. - or Br - After drying, 345.3 g of product was obtained. Analysis showed that the product was high capacity leaching resin-3 (referred to as HCER-3) with surface-bonded polycationic phosphonate, and the water content was about 46.5%. The grafting efficiency was calculated to be about 100%.
[0079] From the surface-bound unsaturated quaternary ammonium cation-bound type described in Examples 1 to 3 The resin is a solid-supported resin with pendant double bonds, and diunsaturated quaternary ammonium cationic phosphonate is used as a grafting monomer. The reverse suspension polymerization method is adopted, and the "graft-from" grafting efficiency reaches 100%.
Claims
1. A method for preparing a high-capacity leaching resin with a surface-bound polycationic phosphonate, which is prepared by the following steps: weighing the surface-bound unsaturated cationic phosphonate, The diunsaturated cationic phosphonate and the aqueous initiator are mixed together in deionized water, stirred and dispersed evenly, swelled at room temperature for 2 to 24 hours under N2 protection, poured into an organic solvent, stirred and dispersed for 0.5 to 2 hours, and then placed in a polymerization kettle, the material temperature in the polymerization kettle is raised to 50 to 90° C., and reverse suspension polymerization is carried out for 2 to 20 hours under stirring, and then the material temperature in the reactor is lowered to room temperature, filtered, washed, and dried to obtain the high-capacity leaching resin of the surface-bonded polycationic phosphonate; The amount of the diunsaturated cationic phosphonate is The amount of the aqueous initiator is 10-1000% of the mass of the di-unsaturated cationic phosphonate, the amount of deionized water is 50-500% of the mass of the di-unsaturated cationic phosphonate, and the amount of the organic solvent is 300-3000% of the mass of the surface-bonded unsaturated cationic polystyrene-based resin; The polystyrene-based resin with unsaturated cationic phosphonate bonded to the surface has a schematic structure of general formula (I) or general formula (II): The diunsaturated cationic phosphonate has a structure shown in the general formula (III) or the general formula (IV): Wherein the general formula (I), general formula (II), general formula (III) or general formula (IV) Refers to polystyrene-based resin, R1 and R2 are selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Hydroxyl, X - Select Cl - Br - or I - One of Refers to C1~C 18 Alkylene or Where n is a natural number between 0 and 2000; The aqueous initiator refers to one of azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, azobisisopropylimidazoline hydrochloride, potassium persulfate or ammonium persulfate; The organic solvent is selected from one or more of toluene, xylene, chlorobenzene, decahydronaphthalene, carbon tetrachloride, 1,2-dichloroethane or petroleum ether with a boiling range of 60 to 90°C.
2. A method for preparing a high-capacity leaching resin with a surface-bound polycationic phosphonate according to claim 1, characterized in that The surface-bound unsaturated cationic phosphonate The specific preparation method is as follows: weigh the solvent and chloromethyl In a reactor, swell at room temperature for 24 hours under N2 protection, then add 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate and a polymerization inhibitor, adjust the temperature of the material in the reactor to 25-45°C, stir and react for 6-16 hours, then increase the reaction temperature to 60-90°C, continue to stir and react for 6-36 hours, and then filter, wash and dry to obtain a surface-bound unsaturated cationic phosphonate of general formula (I) and general formula (II) The amount of solvent used is chloromethylated The amount of the 2-hydroxy-3-(unsaturated tertiary amino)propylphosphonate is 200-2000% by mass. The molar amount of chloromethyl contained is 80-110%, and the amount of the polymerization inhibitor used is 0.1-10% of the weight of 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate; The chloromethylation Refers to chloromethylated polystyrene-based resin; wherein the polystyrene-based resin refers to a cross-linked or non-cross-linked polystyrene resin, or a cross-linked or non-cross-linked (olefin monomer-styrene) copolymer resin; wherein the olefin monomer refers to one or more of vinyl chloride, vinyl acetate, methyl acrylate, ethyl acrylate, butyl acrylate, butadiene or acrylonitrile; The 2-hydroxy-3-(unsaturated tertiary amino)propylphosphonate has a structure shown in the general formula (V) or the general formula (VI): Wherein R1 in the general formula (V) or the general formula (VI) is selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Alkyloxy; The polymerization inhibitor refers to one or more of hydroquinone, p-methoxyphenol, tert-butylhydroquinone, 2,6-dibutylhydroquinone, 2,6-di-tert-butyl-p-cresol or 2,4,6-tri-tert-butylphenol; The solvent is selected from one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, tetrahydrofuran, 1,4-dioxane, 2-methoxyethanol, 2-ethoxyethanol, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.
3. A method for preparing a high-capacity leaching resin with a surface-bound polycationic phosphonate according to claim 1, characterized in that The specific preparation method of the di-unsaturated cationic phosphonate is as follows: weigh a solvent, 2-hydroxy-3-(unsaturated tertiary amino)propyl phosphonate, a dialkylating agent and a polymerization inhibitor respectively in a reaction kettle, raise the temperature of the materials in the reaction kettle to 20-90° C. under N2 protection, stir and react for 6-12 hours, and then filter, wash and dry to obtain a di-unsaturated cationic phosphonate having a structure represented by general formula (III) or general formula (IV); The amount of the solvent is 50-200% of the total mass of the dialkylating agent and 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate, the molar ratio of the dialkylating agent to 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate is 0.48-0.55:1, and the amount of the inhibitor is 0.1-10% of the mass of 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate; The 2-hydroxy-3-(unsaturated tertiary amino)propylphosphonate has a structure shown in the general formula (V) or the general formula (VI): Wherein R1 in the general formula (V) or the general formula (VI) is selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Alkyloxy; The dialkylating agent has a structure shown in general formula (VII): Wherein the general formula (VII) Select C1~C 18 Alkylene or Where n is a natural number between 0 and 2000, and X is one of Cl, Br or I; The polymerization inhibitor refers to one or more of hydroquinone, p-methoxyphenol, tert-butylhydroquinone, 2,6-dibutylhydroquinone, 2,6-di-tert-butyl-p-cresol or 2,4,6-tri-tert-butylphenol; The solvent is selected from one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, tetrahydrofuran, 1,4-dioxane, 2-methoxyethanol, 2-ethoxyethanol, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.
4. A method for preparing a high-capacity leaching resin having a surface-bound polycationic phosphonate according to claim 2 or 3, characterized in that The 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonate is prepared by the following method: weighing a phosphite ester and putting it into a reactor, adding sodium alcoholate under N2 protection and stirring, then raising the temperature of the material in the reactor to 70-140° C., continuously adding N-glycidyl-N,N-diallylamine or N-glycidyl-N-alkyl-N-allylamine to the reactor, stirring and reacting for 8-12 hours, and separating and purifying to obtain 2-hydroxy-3-(unsaturated tertiary amino) propyl phosphonic acid dialkyl ester; The amount of the phosphite is 2 to 10 times the weight of N-glycidyl-N,N-diallylamine or N-glycidyl-N-alkyl-N-allylamine, and the amount of the sodium alkoxide is 0.5 to 5% of the weight of N-glycidyl-N,N-diallylamine or N-glycidyl-N-alkyl-N-allylamine; The N-glycidyl-N-alkyl-N-allylamine has a structure shown in the general formula (VIII): The hydrocarbon group refers to R1 in the general formula (VIII), and R1 is selected from C1 to C 18 Hydrocarbon; The phosphite has a structure shown in the general formula (IX): Wherein R2 in the general formula (IX) is selected from C1 to C 18 Hydrocarbon, R3 is selected from C1~C 18 Hydrocarbon or C1~C 18 Alkyloxy; The sodium alkoxide refers to one of sodium methoxide, sodium ethoxide, sodium propoxide or sodium butoxide.