A preparation method and application of MQ resin
Through a new MQ resin preparation method, the low vinyl MQ resin is re-captured by a capping agent to form a double-layer spherical structure, which solves the low light transmittance, low peeling force and aging of the silicone pressure-sensitive adhesive. The problem of poor peeling force stability improves the performance of pressure-sensitive adhesives and avoids silicon transfer. It is suitable for high-end optical fields.
Patent Information
- Application Number
- CN202410320651.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-03-20
AI Technical Summary
In the prior art, silicone pressure-sensitive adhesives have low light transmittance, low peeling force and poor peeling force stability after aging, and silicon transfer is prone to problems during use.
Through a preparation method of an MQ resin, it includes adding solvent, deionized water and acidic catalyst to the reaction vessel, stirring evenly, adding ethyl orthosilicate, followed by adding capping agent and extraction agent, and leaving the layering on standstill to obtain low ethylene The base MQ resin solution is then added with an alkaline catalyst for high-temperature reflux reaction, water molecules are eliminated and neutralized, and finally, low boiling substances are removed by decompression to obtain a low vinyl content and low hydroxyl value MQ resin. This method re-capsulates the low vinyl MQ resin through a capping agent to form a double-layer spherical structure, replacing the traditional anchoring agent and improving the performance of the pressure-sensitive adhesive.
It effectively improves the peel strength, light transmittance and aging adhesion stability of silicone pressure-sensitive adhesive, solves the silicon transfer problem, and is suitable for high-end optical applications.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic silicon resins, and in particular to a preparation method of MQ resin and application thereof. Background Art
[0002] At present, as a silicone adhesive, silicone pressure-sensitive adhesive has better high and low temperature resistance (long-term use within -50℃ ~ 200℃), chemical resistance (solvent resistance) and low dielectric properties compared to traditional pressure-sensitive adhesives, and also has good adhesion to low surface energy materials. This makes silicone pressure-sensitive adhesive tapes widely used in industrial production and the electronics industry in the form of splicing tapes, electrical tapes, masking tapes, protective films, etc. Silicone pressure-sensitive adhesive is mainly made by mixing silicone rubber raw rubber, MQ silicone resin and solvent in a certain proportion. Silicone rubber can increase the fluidity of pressure-sensitive adhesive, thereby increasing the interfacial adhesion, and has strong initial adhesion, serving as the main body of cross-linking and curing. MQ silicone resin, as a reinforcing agent, has a greater influence on the bonding properties of pressure-sensitive adhesives. The bonding strength of silicone pressure-sensitive adhesives can be significantly improved by tackifying and reinforcing with MQ silicone resin. As market competition intensifies, people have put forward more stringent requirements on the performance of silicone pressure-sensitive adhesives, such as: higher peel strength of silicone pressure-sensitive adhesives (>1000g / inch), stronger high and low temperature resistance (-75~260℃), lower silicon transfer and high light transmittance requirements; and an important way to improve the performance of silicone pressure-sensitive adhesives is to improve the performance of MQ silicone resin and anchoring agent. The commercially available anchoring agents are usually small molecular monomers with poor stability and high volatility, which are easy to migrate and contaminate the surface of the adherend.
[0003] Conventional commercially available methyl MQ resins have high hydroxyl content and poor compatibility, which leads to low peel force and poor peel force stability after aging in the prepared pressure-sensitive adhesive samples. Vinyl MQ resins mostly have a vinyl content of more than 2wt%. A small amount is added to improve the cohesive strength of the pressure-sensitive adhesive, but it cannot replace methyl MQ resin as an independent tackifying resin material.
[0004] In addition, since conventional MQ resin has poor compatibility with silicone oil and silicone rubber systems, adding it to pressure-sensitive adhesives will reduce the light transmittance, thereby affecting its application in high-end optical fields.
[0005] In summary, the pressure-sensitive adhesive obtained by adding MQ resin to the silicone oil and silicone rubber system in the prior art has low light transmittance, low peel force and poor peel force stability after aging, and silicone transfer is prone to occur during use. Summary of the invention
[0006] The purpose of the present invention is to overcome the above technical deficiencies, provide a preparation method of MQ resin and its application, and solve the technical problems of low light transmittance, low peel force and poor peel force stability after aging of pressure-sensitive adhesives in the prior art, and silicon transfer during use.
[0007] In order to achieve the above technical purpose, the technical solution of the present invention provides a method for preparing MQ resin, comprising the following steps:
[0008] (1) adding a solvent, deionized water and an acidic catalyst into a reaction vessel, stirring evenly, adding ethyl orthosilicate, stirring evenly, and reacting for 0.2-1h; adding a type of end-capping agent to the reaction solution of the above reaction, reacting at 25-40° C. for 1-4h; adding an extractant, standing and stratifying, retaining the upper organic phase, and obtaining a low vinyl MQ resin solution;
[0009] (2) adding the second type of end-capping agent and the alkaline catalyst to the low vinyl MQ resin solution, subjecting the solution to a high temperature reflux reaction, and removing the generated water molecules in the system until no water is produced; adding an acid to neutralize the solution, and washing the solution with water until it is neutral, taking the upper organic phase solution, and removing the low boiling point by decompression to obtain the MQ resin.
[0010] Furthermore, the addition amount of each substance in step (1) is calculated by mass fraction as follows:
[0011] 100 parts of tetraethyl orthosilicate;
[0012] 1-10 parts of a capping agent type A, preferably 2-6 parts;
[0013] 40-80 parts of a capping agent of type B, preferably 50-70 parts;
[0014] 0.5-2 parts of acidic catalyst, preferably 0.7-1.5 parts;
[0015] 30-70 parts of deionized water, preferably 40-60 parts;
[0016] 50-100 parts of solvent, preferably 60-80 parts;
[0017] Furthermore, the addition amount of each substance in step (2) is calculated by mass fraction as follows:
[0018] 100 parts of MQ resin solution (without solvent);
[0019] 10-30 parts of the second type of capping agent, preferably 15-25 parts;
[0020] 0.2-1 part of basic catalyst, preferably 0.4-0.8 part;
[0021] Furthermore, the acidic catalyst in step (1) is one or more of formic acid, acetic acid, hydrochloric acid, fluorosulfonic acid, sulfuric acid, hydrobromic acid, hydrofluoric acid, and p-toluenesulfonic acid, preferably hydrochloric acid;
[0022] Further, the solvent in step (1) includes any one or more of methanol, ethanol, n-propanol, and isopropanol, preferably ethanol;
[0023] Furthermore, the type of end-capping agent in step (1) includes end-capping agent A and end-capping agent B, wherein end-capping agent A is one or more of vinyldimethylethoxysilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and tetramethyldivinyldisiloxane, and end-capping agent B is one or more of methoxytrimethylsilane, ethoxytrimethylsilane, dimethoxydimethylsilane, diethoxydimethylsilane, methyltrimethoxysilane, methyltriethoxysilane, and hexamethyldisiloxane, preferably a mixture of tetramethyldivinyldisiloxane and hexamethyldisiloxane.
[0024] Furthermore, the extractant in step (1) is any one or more of cyclohexane, toluene, and xylene, preferably toluene;
[0025] Furthermore, the second type of end-capping agent in step (2) is one or more of methoxytrimethylsilane, trimethylethoxysilane, and trimethylchlorosilane, preferably methoxytrimethylsilane;
[0026] Furthermore, the alkaline catalyst in step (2) is one or more of potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, and triethylamine, preferably tetramethylammonium hydroxide;
[0027] The MQ resin obtained by the present invention is a low vinyl content and low hydroxyl value MQ resin, and its structural formula is as follows:
[0028]
[0029] Wherein, M is vinyl, hydroxyl, alkoxy and trimethylsiloxane; the ratio of the number of siloxane units to tetraphenylsiloxane units in the MQ resin structure, M / Q, is 0.6-1.0, preferably 0.7-0.9; the weight average molecular weight of the MQ resin is 3000-9000, preferably 4000-8000; the vinyl content is 0.02-0.24%, preferably 0.04-0.15%, and the hydroxyl content is 0.3-2.0wt%, preferably 0.5-1.5wt%.
[0030] Furthermore, the second type of end-capping agent in step (2) is one or more of γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, γ-(methacryloxy)propyltrimethoxysilane, γ-(methacryloxy)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane and aminophenylpropyltrimethoxysilane, preferably γ-glycidyloxypropyltrimethoxysilane.
[0031] The MQ resin obtained by the present invention is a low vinyl content and low hydroxyl value modified MQ resin, and its structural formula is as follows:
[0032]
[0033] Wherein, M is one or more of vinyl, trimethylsiloxane, hydroxyl, alkoxy, epoxy, acetoxy, and amino, preferably vinyl, trimethoxysiloxane, hydroxyl, and epoxy; the ratio of the number of siloxane units to tetraphenylsiloxane units in the MQ resin structure is 0.6-1.0, preferably 0.7-0.9; the weight average molecular weight of the MQ resin is 3000-9000, preferably 4000-8000; the vinyl content is 0.02-0.24%, preferably 0.04-0.15%, the hydroxyl content is 0.3-2.0wt%, preferably 0.5-1.5wt%. The content of functional groups (such as epoxy, alkoxy, acetoxy, amino, etc.) is 0.3-1.5%, preferably 0.5-1.0%.
[0034] An application based on the MQ resin described above comprises the following steps: preparing a pressure-sensitive adhesive by mixing the modified MQ resin with low vinyl content and low hydroxyl value as an anchoring agent with methyl vinyl silicone rubber, vinyl silicone oil, hydrogen-containing silicone oil, an inhibitor, a platinum catalyst and a solvent; and coating the pressure-sensitive adhesive on a substrate to obtain a pressure-sensitive adhesive product.
[0035] The substrate can be selected from one of TPU, PET, CPP and BOPP; the molecular weight of the methyl vinyl silicone rubber is 400,000-700,000, the vinyl content is 0.1wt%-0.5wt%, the hydrogen content of the hydrogen-containing silicone oil can be selected as 0.8wt%-1.6wt%, and the volatile content is ≤2.0%; the commercially available anchoring agent is Dow Corning 297, the inhibitor is acetylene cyclohexanol, and the catalyst is a 5000ppm platinum catalyst.
[0036] The beneficial effects of the present invention include: the present invention provides a method for preparing MQ resin, the operation method is simple, the conditions are mild, the low vinyl MQ resin is re-end-capped by an end-capping agent, and the end-capped product is a double-layer spherical structure of low vinyl content and low hydroxyl value MQ resin or low vinyl content and low hydroxyl value modified MQ resin, which overcomes the problem of high hydroxyl content in silicone resin prepared by the prior art, and can replace the compound system of vinyl MQ resin and methyl MQ resin in the field of organic silicon pressure-sensitive adhesive, which is conducive to large-scale production. The MQ resin effectively improves the peel strength, light transmittance and aging adhesion stability of the organic silicon pressure-sensitive adhesive.
[0037] The prepared low-vinyl content and low-hydroxyl value modified MQ resin introduces functional monomers (such as epoxy, alkoxy, acetoxy, amino, etc.) into the low-vinyl MQ resin to replace the anchoring agent in the prior art. On the basis of satisfying the requirement of improving the adhesion of the substrate, it solves the problem of silicon transfer of the pressure-sensitive adhesive during long-term use.
[0038] The pressure-sensitive adhesive provided by the invention is coated on a substrate and cured at 120° C.-160° C. (60-120 seconds). The pressure-sensitive adhesive product prepared by the invention has high peeling strength, aging adhesion stability and light transmittance. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] Sources of raw materials in the following examples: all purchased from Aladdin.
[0041] The molecular weight and its distribution test method in the examples are measured by gel permeation chromatography (GPC) using toluene as the mobile phase.
[0042] Test method for silanol content of MQ resin sample: Nuclear magnetic resonance silicon spectrum.
[0043] Pressure sensitive adhesive sample preparation and test method:
[0044] 1. Glue making: It is composed of MQ resin, vinyl methyl silicone rubber, hydrogen-containing silicone oil, inhibitor, anchoring agent, platinum catalyst and solvent.
[0045] 2. Sample preparation: Use a 70-micron coating rod to evenly coat the mixed pressure-sensitive adhesive sample on the corona-treated PET film, bake it in a 150°C oven for 2 minutes, and then cut it into tapes and stick them on the steel plate.
[0046] 3. Test: According to GB / T 2792-2014 method, use a tensile testing machine to test the peeling force of the pressure-sensitive adhesive.
[0047] 4. Aging: The samples were aged for 72 hours in a constant temperature and humidity chamber at 85°C / 85%RH, and then the peeling strength after aging was tested.
[0048] 5. Light transmittance: Tested with a light transmittance haze tester;
[0049] 6. Silicon transfer: The sample is aged in a constant temperature and humidity chamber at 85°C / 85%RH for 72 hours, and the contamination state of the adherend surface is observed.
[0050] Example 1
[0051] Add 210g water, 200g isopropanol and 2.0g concentrated hydrochloric acid to the reactor, stir evenly, add 400g ethyl orthosilicate to the reactor A, the temperature is 25°C, stir and react for 10min, add 320g hexamethyldisiloxane and 4g tetramethyldivinyldisiloxane, the temperature is 25°C, react for 2h, add 300g toluene, stir evenly and let stand for stratification, add sodium bicarbonate to neutralize, retain the upper organic phase MQ resin solution; add 70g trimethylethoxysilane and 1.8g sodium hydroxide, 110°C high temperature reflux reaction for 2h, remove the generated water molecules in the system until no water is produced; add hydrochloric acid to neutralize, wash with water to neutrality, take the upper organic phase solution, and reduce the pressure to obtain a low vinyl content and low hydroxyl value MQ resin. The M / Q ratio of the test sample is 1.0, the weight average molecular weight is 3385, the hydroxyl content is 2.0wt%, and the vinyl content is 0.02wt%. Take 40 g of the MQ powder sample and stir evenly with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogenated silicone oil, 0.6 g of commercially available anchoring agent, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm to obtain a silicone pressure-sensitive adhesive component sample 1.
[0052] The hexamethyldisiloxane in this example is replaced by an equal amount of methoxytrimethylsilane or ethoxytrimethylsilane; the tetramethyldivinyldisiloxane is replaced by an equal amount of vinyldimethylmethoxysilane or vinyldimethylethoxysilane; and the trimethylethoxysilane is replaced by an equal amount of methoxytrimethylsilane or trimethylchlorosilane. The performance of the prepared silicone pressure-sensitive adhesive is similar to that of Sample 1.
[0053] Example 2
[0054] Add 280g water, 200g isopropanol and 8.0g concentrated hydrochloric acid to the reactor, stir evenly, add 400g ethyl orthosilicate to the reactor A, the temperature is 25°C, stir and react for 10min, add 160g hexamethyldisiloxane and 40g tetramethyldivinyldisiloxane, the temperature is 25°C, react for 2h, add 300g toluene, stir evenly and let stand for stratification, add sodium bicarbonate to neutralize, retain the upper organic phase MQ resin solution; add 120g trimethylethoxysilane and 4.0g sodium hydroxide, reflux at 110°C for 2h, remove the generated water molecules in the system until no water is produced; add hydrochloric acid to neutralize, wash with water to neutrality, take the upper organic phase solution, and reduce the pressure to obtain a low vinyl content and low hydroxyl value MQ resin. The M / Q ratio of the test sample is 0.60, the weight average molecular weight is 8985, the hydroxyl content is 1.50wt%, and the vinyl content is 0.24wt%. Take 40 g of the MQ powder sample and mix it with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogenated silicone oil, 0.6 g of commercially available anchoring agent, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm, and stir evenly to obtain a silicone pressure-sensitive adhesive component sample 2.
[0055] Example 3
[0056] Add 160g water, 320g isopropanol and 6.0g concentrated hydrochloric acid to the reactor, stir evenly, add 400g ethyl orthosilicate to the reactor A, the temperature is 25°C, stir and react for 10min, add 280g hexamethyldisiloxane and 8.0g tetramethyldivinyldisiloxane, the temperature is 25°C, react for 2h, add 300g toluene, stir evenly and let stand for stratification, add sodium bicarbonate to neutralize, retain the upper organic phase MQ resin solution; add 60g trimethylethoxysilane and 1.6g sodium hydroxide, reflux at 110°C for 2h, remove the generated water molecules in the system until no water is produced; add hydrochloric acid to neutralize, wash with water to neutrality, take the upper organic phase solution, and reduce the pressure to obtain a low vinyl content and low hydroxyl value MQ resin. The M / Q ratio of the test sample is 0.70, the weight average molecular weight is 7985, the hydroxyl content is 0.52wt%, and the vinyl content is 0.04wt%. Take 40 g of the MQ powder sample and stir evenly with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogenated silicone oil, 0.6 g of commercially available anchoring agent, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm to obtain a silicone pressure-sensitive adhesive component sample 3.
[0057] Example 4
[0058] Add 200g water, 280g isopropanol and 4.2g concentrated hydrochloric acid to the reactor, stir evenly, add 400g ethyl orthosilicate to the reactor A, the temperature is 25℃, stir and react for 10min, add 240g hexamethyldisiloxane and 16g tetramethyldivinyldisiloxane, the temperature is 35℃, react for 2h, add 300g toluene, reflux for 2h; stop stirring, let stand for stratification, add sodium bicarbonate to neutralize, retain the upper organic phase MQ resin solution; add 100g trimethylethoxysilane and 1g potassium hydroxide, reflux at 110℃ for 2h, remove the generated water molecules in the system until no water is produced; add hydrochloric acid to neutralize, wash with water to neutrality, take the upper organic phase solution, and reduce the pressure to obtain a low vinyl content and low hydroxyl value MQ resin. The M / Q ratio of the test sample is 0.71, the weight average molecular weight is 5964, the hydroxyl content is 0.94wt%, and the vinyl content is 0.09wt%. Take 40 g of the MQ powder sample and mix it with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogenated silicone oil, 0.6 g of commercially available anchoring agent, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm, and stir evenly to obtain a silicone pressure-sensitive adhesive component sample 4.
[0059] Example 5
[0060] Add 240g water, 240g isopropanol and 2.8g concentrated hydrochloric acid to the reactor, stir evenly, add 400g ethyl orthosilicate to the reactor A, stir and react for 60min, add 200g hexamethyldisiloxane and 24g tetramethyldivinyldisiloxane, react for 4h at 25℃, add 200g toluene, reflux for 2h; stop stirring, let stand for stratification, add sodium bicarbonate to neutralize, retain the upper organic phase MQ resin solution; add 80g trimethylethoxysilane and 1g tetramethylammonium hydroxide, reflux at 110℃ for 2h, remove the generated water molecules in the system until no water is produced; add hydrochloric acid to neutralize, wash with water to neutrality, take the upper organic phase solution, and decompress to obtain a low vinyl content and low hydroxyl value MQ resin. The M / Q ratio of the test sample is 0.77, the weight average molecular weight is 4012, the hydroxyl content is 0.61wt%, and the vinyl content is 0.14wt%. Take 40 g of the MQ powder sample and mix it with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogenated silicone oil, 0.6 g of commercially available anchoring agent, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm, and stir evenly to obtain a silicone pressure-sensitive adhesive component sample 5.
[0061] Example 6
[0062] Add 180g of water, 250g of isopropanol and 6.2g of concentrated hydrochloric acid to the reactor and stir evenly. Add 400g of tetraethyl orthosilicate to the reactor A and stir to react for 30min. Add 285g of hexamethyldisiloxane and 15g of tetramethyldivinyldisiloxane and react at 35°C for 1h. Add 200g of toluene and reflux for 2h. Stop stirring, let stand for stratification, add sodium bicarbonate for neutralization, and retain the upper organic phase MQ resin solution. Add 72g of γ-glycidyloxypropyltrimethoxysilane and 1g of tetramethylammonium hydroxide, reflux for 2h at 110°C, and remove the generated water molecules in the system until no water is produced. Add hydrochloric acid for neutralization, wash with water until neutral, take the upper organic phase solution, and decompress and degas to obtain a low vinyl content and low hydroxyl value modified MQ resin. The tested sample had an M / Q ratio of 0.81, a weight average molecular weight of 5312, a hydroxyl content of 0.56 wt %, a vinyl content of 0.08 wt %, and an epoxy content of 0.78 wt %.
[0063] Take 1 g of the low vinyl content and low hydroxyl value modified MQ resin powder sample prepared in this example, 40 g of the MQ resin sample synthesized in Example 2, 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogen-containing silicone oil, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm, and stir evenly to obtain a silicone pressure-sensitive adhesive component sample 6.
[0064] The γ-glycidyloxypropyltrimethoxysilane in this example is replaced by an equal amount of one of γ-glycidyloxypropyltriethoxysilane, γ-(methacryloxy)propyltrimethoxysilane, γ-(methacryloxy)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane and aminophenylpropyltrimethoxysilane, and the performance of the prepared silicone pressure-sensitive adhesive sample is similar to that of Sample 6.
[0065] Example 7
[0066] Take 40 g of commercially available methyl MQ resin (molecular weight 3822, hydroxyl content 0.52%) sample and stir evenly with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogen-containing silicone oil, 0.6 g of low vinyl content and low hydroxyl value modified MQ resin synthesized in Example 6, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm to obtain silicone pressure-sensitive adhesive component sample 7.
[0067] Comparative Example 1
[0068] Take 40 g of commercially available methyl MQ resin (molecular weight 3822, hydroxyl content 0.52%) sample and mix with 20 g of commercially available vinyl methyl silicone rubber from the same batch, 60 g of xylene, 0.8 g of hydrogen-containing silicone oil, 0.6 g of commercial anchoring agent, 0.1 g of ethynyl cyclohexanol, and 0.4 g of a catalyst with a platinum content of 5000 ppm, and stir evenly to obtain silicone pressure-sensitive adhesive component sample 8.
[0069] Comparative Example 2
[0070] Take 60 g of commercially available Dow Corning pressure-sensitive adhesive 7657, 40 g of xylene, 0.8 g of hydrogen-containing silicone oil, 0.6 g of commercially available anchoring agent, and 0.4 g of a catalyst with a platinum content of 5000 ppm, and stir evenly to obtain a silicone pressure-sensitive adhesive component sample 9.
[0071] The silicone pressure-sensitive adhesive component samples 1-9 were taken for pressure-sensitive adhesive performance testing, and the test results are shown in the following table.
[0072]
[0073]
[0074] From the results, we can see that by reducing the ethylene and hydroxyl contents of MQ resin, the problems of low peel force and poor peel force stability after aging can be solved. At the same time, introducing a small amount of vinyl into MQ resin can significantly improve the light transmittance of pressure-sensitive adhesive products. The low-hydroxyl and low-vinyl modified MQ resin synthesized by the same method can replace the traditional anchoring agent and solve the technical problem that silicon is easy to migrate and contaminate the surface of the adherend during the long-term use of pressure-sensitive adhesives.
[0075] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. The application of MQ resin in pressure-sensitive adhesive is characterized in that: The following steps are involved: Mixing low-vinyl-content low-hydroxyl-value MQ resin as a tackifying resin, low-vinyl-content low-hydroxyl-value modified MQ resin as an anchoring agent with methyl vinyl silicone rubber, hydrogen-containing silicone oil, an inhibitor, a platinum catalyst, and a solvent to prepare an organic silicone pressure-sensitive adhesive; coating the organic silicone pressure-sensitive adhesive on a substrate to obtain a pressure-sensitive adhesive product; The preparation method of the low vinyl content and low hydroxyl value MQ resin or the low vinyl content and low hydroxyl value modified MQ resin comprises the following steps: (1) adding a solvent, deionized water and an acidic catalyst into a reaction vessel, stirring evenly, adding ethyl orthosilicate, stirring evenly, and reacting for 0.2-1h; adding a type of end-capping agent to the reaction solution of the above reaction, reacting at 25-40° C. for 1-4h; adding an extractant, standing and stratifying, retaining the upper organic phase, and obtaining an MQ resin solution; The first type of end-capping agent is a mixture of an end-capping agent A and an end-capping agent B, wherein the end-capping agent A is one or more of vinyldimethylmethoxysilane, vinyldimethylethoxysilane, and tetramethyldivinyldisiloxane, and the end-capping agent B is one or more of trimethylmethoxysilane, trimethylethoxysilane, trimethylchlorosilane, and hexamethyldisiloxane; The addition amount of each substance is respectively: 100 parts of tetraethyl orthosilicate, 1-10 parts of end-capping agent A, 40-80 parts of end-capping agent B, and 0.5-2 parts of acid catalyst; (2) adding the second type of end-capping agent and the alkaline catalyst to the MQ resin solution, and subjecting the solution to a high temperature reflux reaction for 2-6 hours to remove the generated water molecules in the system; after the reaction is completed, adding an acid for neutralization, and washing with water until neutral, taking the upper organic phase solution, and removing the low-boiling substances by decompression to obtain the MQ resin; The second type of end-capping agent is one or more of methoxytrimethylsilane, trimethylethoxysilane, and trimethylchlorosilane, and the prepared MQ resin is a low-vinyl content and low-hydroxyl value MQ resin; The second type of end-capping agent is one or more of γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, γ-(methacryloxy)propyltrimethoxysilane, γ-(methacryloxy)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane and aminophenylpropyltrimethoxysilane. The prepared MQ resin is a low vinyl content and low hydroxyl value modified MQ resin.
2. The use according to claim 1, characterized in that: The acid catalyst is one or more of formic acid, acetic acid, hydrochloric acid, fluorosulfonic acid, sulfuric acid, hydrobromic acid, hydrofluoric acid, and p-toluenesulfonic acid.
3. The use according to claim 1, characterized in that: In step (2), the added amounts of the substances are as follows: 100 parts of MQ resin solution, 10-30 parts of the second type capping agent, and 0.2-1 part of the alkaline catalyst, respectively.
4. The use according to claim 1, characterized in that: The alkaline catalyst is one or more of potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide and triethylamine.
Citation Information
Patent Citations
Solvent-free organic silicon pressure-sensitive adhesive and preparation method thereof
CN102174309A
Vinyl MQ silicon resin and preparation method thereof
CN102775612A
Modified MQ (mono-quad) resin, synthesis method and application on pressure sensitive adhesive
CN110760068A
Cited By
Modified MQ type silicon resin as well as preparation method and application thereof
CN120230291A