A colorless and transparent phenolic resin adhesive and preparation method thereof

Through the combination of modified monomers and reinforcing fillers, hyperbranched phenolic resin molecules and dynamic cross-linked structures are formed, which solves the problem of brittleness of phenolic resin adhesives and significantly improves its toughness and impact resistance.

CN118085780BActive Publication Date: 2024-10-01ZHEJIANG ANYI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410332083.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-10-01
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

Due to its short flexible chain and high brittleness, traditional phenolic resin adhesives are prone to cracks after being impacted, which affects the bonding effect and limits its application.

Method used

By preparing modified monomers and reinforcing fillers, hyperbranched silicone segments and dynamic cross-linked structures are formed in the phenolic resin molecules, combined with multi-layer dynamic covalent bonds of cellulose and hexagonal boron nitride, to enhance the toughness of the resin.

Benefits of technology

Significantly improves the toughness of phenolic resin adhesive, which can buffer energy through the breaking and reorganization process of dynamic covalent bonds after being impacted, and enhance impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a colorless and transparent phenolic resin adhesive and a preparation method thereof. The method specifically comprises the following steps: weighing the following raw materials in parts by weight: 60-80 parts of phenol, 30-40 parts of a modified monomer, 180-230 parts of a formaldehyde solution, 3-5 parts of a sodium hydroxide solution and 5-10 parts of a reinforcing filler; mixing and stirring the phenol, the modified monomer and the sodium hydroxide solution; heating the mixture, adding the formaldehyde solution and the reinforcing filler, and reacting the mixture to obtain the phenolic resin adhesive; the modified monomer is a hyperbranched organic silicon segment structure, so that the prepared phenolic resin molecule is hyperbranched and can form a dynamic crosslink with the reinforcing filler, so that the brittleness of the prepared phenolic resin adhesive is reduced; and through multiple layers of dynamic covalent bonds, after the phenolic resin adhesive is impacted, the breaking and reorganization process of the dynamic covalent bonds can dissipate a large amount of energy, thereby playing a role of buffering energy absorption and impact resistance, thereby enhancing the toughness of the phenolic resin adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive preparation, and in particular to a colorless and transparent phenolic resin adhesive and a preparation method thereof. Background Art

[0002] Phenolic resin is a resin made by polycondensation of phenol and formaldehyde under catalyst conditions, neutralization and water washing. Phenolic resin is a representative of thermosetting resins. Phenolic resin has the advantages of good bonding properties, water resistance, heat resistance, chemical resistance, etc., especially in the production of water-resistant and weather-resistant outdoor wood products. It has incomparable advantages over urea-formaldehyde resin, so it is widely used in the wood-based panel industry. Its usage is very large, second only to urea-formaldehyde resin. However, due to the defects of its own molecular structure and preparation method, traditional unmodified phenolic resin has a short flexible chain, and adjacent benzene rings are only connected by methylene, making it rigid and poor in flexibility. After the prepared adhesive is cured, it will crack when subjected to a slight impact, which reduces the bonding effect and causes the product to be unable to be used normally, seriously affecting the application of phenolic resin adhesives. Summary of the invention

[0003] The purpose of the present invention is to provide a colorless and transparent phenolic resin adhesive and a preparation method thereof, so as to solve the problem that the phenolic resin adhesive at present is very brittle and cracks appear after being impacted, which affects the normal use.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a colorless and transparent phenolic resin adhesive comprises the following steps:

[0006] Step A1: γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane and deionized water are mixed, stirred for 10-15 minutes at a speed of 200-300 r / min and a temperature of 60-70° C., concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added, and the reaction is carried out for 4-6 hours, and the pH is adjusted to neutral to obtain intermediate 1;

[0007] Step A2: Tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and DMF are mixed evenly, stirred at a speed of 150-200 r / min and a temperature of 50-60° C., chloroplatinic acid is added, and the reaction is carried out for 6-8 hours, p-hydroxystyrene is added, and the reaction is continued for 8-10 hours to obtain intermediate 2, intermediate 2, 4-formylphenylboronic acid and DMF are mixed evenly, stirred at a speed of 120-150 r / min and a temperature of 45-55° C., sodium cyanoborohydride is added, and the reaction is carried out for 20-25 hours to obtain a modified monomer;

[0008] Step A3: Weigh the following raw materials in parts by weight: 60-80 parts of phenol, 30-40 parts of modified monomer, 180-230 parts of formaldehyde solution, 3-5 parts of sodium hydroxide solution and 5-10 parts of reinforcing filler, mix the phenol, modified monomer and sodium hydroxide solution evenly, stir for 20-30 minutes at a speed of 120-150r / min and a temperature of 80-85°C, raise the temperature to 90-95°C, add the formaldehyde solution and reinforcing filler, and react for 1-1.5 hours to obtain a phenolic resin adhesive.

[0009] Furthermore, the amount ratio of γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane, deionized water and 1,1,3,3-tetramethyldisiloxane described in step A1 is 1mmol:2mmol:20mL:1.5mmol, and the amount of concentrated sulfuric acid is 2% of the mass of γ-aminopropylmethyldiethoxysilane.

[0010] Furthermore, the molar ratio of tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and p-hydroxystyrene described in step A2 is 1:4:4, the amount of chloroplatinic acid is 1‰ of the mass of tetramethyltetravinylcyclotetrasiloxane, the molar ratio of the amino group on intermediate 2 and 4-formylphenylboric acid is 1:1, and the amount of sodium cyanoborohydride is 3% of the mass of intermediate 2.

[0011] Furthermore, the mass fraction of the sodium hydroxide solution described in step A3 is 40%, and the mass fraction of the formaldehyde solution is 37%.

[0012] Further, the reinforcing filler is prepared by the following steps:

[0013] Step B1: adding cellulose to a sodium hydroxide solution, reacting for 3-5 hours at a speed of 120-150 r / min and a temperature of 50-55° C., filtering the filtrate, washing to neutrality, and obtaining alkalized cellulose; uniformly mixing the alkalized cellulose, epichlorohydrin and dioxane, stirring and adding sodium hydroxide at a speed of 60-80 r / min and a temperature of 35-40° C., and reacting for 2-4 hours to obtain pretreated cellulose; uniformly mixing the pretreated cellulose, furfurylamine and DMF, and reacting for 3-5 hours at a speed of 120-150 r / min, a temperature of 30-40° C. and a pH value of 10-11, and obtaining modified cellulose;

[0014] Step B2: Mix hexagonal boron nitride, urea and deionized water evenly, grind for 10-15h, filter and remove the filtrate, disperse the substrate in ethanol, add 3-isocyanatepropyltrimethoxysilane, react for 3-5h at a speed of 120-150r / min and a temperature of 40-50°C to obtain pretreated hexagonal boron nitride, dissolve maleic anhydride in toluene, stir and add 3-aminopropyltriethoxysilane at a speed of 150-200r / min and a temperature of 50-55°C, react for 1-1.5h, add sodium acetate and hydroquinone, heat to 110-115°C, reflux for 2-3h to obtain a modifier;

[0015] Step B3: Disperse the pretreated hexagonal boron nitride in dimethyl sulfoxide, add a modifier, react for 10-15 hours at a speed of 120-150 r / min and a temperature of 60-65°C, cool to 20-25°C, add ammonium fluoride, react for 20-25 hours to obtain modified hexagonal boron nitride, mix the modified hexagonal boron nitride, modified cellulose and DMF, react for 8-10 hours at a speed of 200-300 r / min and a temperature of 20-25°C, filter and remove the filtrate and dry to obtain a reinforcing filler.

[0016] Furthermore, the dosage ratio of cellulose and sodium hydroxide solution in step B1 is 1g:10mL, the mass fraction of sodium hydroxide solution is 4%, the dosage ratio of alkalized cellulose, epichlorohydrin and sodium hydroxide is 1g:25mL:5g, and the molar ratio of epoxy group and furfurylamine on pretreated cellulose is 1:1.

[0017] Further, the amount ratio of hexagonal boron nitride, urea, deionized water and 3-isocyanatepropyltrimethoxysilane described in step B2 is 1g:30g:30mL:3mL, the molar ratio of maleic anhydride and 3-aminopropyltriethoxysilane is 1:1, the amount of sodium acetate is 5% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane, and the amount of hydroquinone is 0.7% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane.

[0018] Furthermore, the mass ratio of the pretreated hexagonal boron nitride, the modifier and the ammonium fluoride in step B3 is 2:2.5:0.3, and the mass ratio of the modified hexagonal boron nitride and the modified cellulose is 1:6.

[0019] Beneficial effects of the invention: The colorless and transparent phenolic resin adhesive disclosed in the invention comprises the following raw materials: phenol, modified monomer, formaldehyde solution, sodium hydroxide solution and reinforcing filler. When reinforcing filler is added, the boric acid group on the side chain of the modified monomer can form borate with the hydroxyl group on the surface of the reinforcing filler, thereby forming a core-shell structure in which the phenolic resin molecule encapsulates the reinforcing filler, thereby increasing the toughness of the phenolic resin adhesive. The modified monomer is first hydrolyzed with γ-aminopropylmethyldiethoxysilane and diphenyldichlorosilane as raw materials, and then condensed with 1,1,3,3-tetramethyldisiloxane to form a diisocyanate containing amino groups on the side chain. The intermediate 1 is prepared by reacting the intermediate 1 with tetramethyltetravinylcyclotetrasiloxane under the action of chloroplatinic acid and controlling the dosage, so that the Si-H bond on the intermediate 1 reacts with the double bond on the tetramethyltetravinylcyclotetrasiloxane to form Si-H termination, and then reacting with p-hydroxystyrene to prepare the intermediate 2, and the intermediate 2 is reacted with 4-formylphenylboronic acid, so that the amino group on the intermediate 2 reacts with the aldehyde group on the 4-formylphenylboronic acid to prepare the modified monomer, and the modified monomer is a hyperbranched organic silicon segment structure, so that the prepared phenolic resin molecule is hyperbranched and can be combined with the reinforcing filler to form a phenolic resin. The cellulose is treated with sodium hydroxide to form alkalized cellulose, and the alkalized cellulose is reacted with epichlorohydrin to make the epichlorohydrin first open the ring and then close the ring to obtain pretreated cellulose. The pretreated cellulose is reacted with furfurylamine to make the epoxy group on the pretreated cellulose react with the amino group on the furfurylamine to obtain modified cellulose. The hexagonal boron nitride is treated with urea to make the surface of the hexagonal boron nitride amino, and then reacted with 3-isocyanate propyltrimethoxysilane to make the surface grafted with siloxane structure. Maleic anhydride and 3-aminopropyl triethoxysilane are reacted with 1,2-dimethoxy- ... The pretreated hexagonal boron nitride and the modifier are hydrolyzed and condensed to form a cage-type silsesquioxane on the surface of the pretreated hexagonal boron nitride. The cage-type silsesquioxane contains a maleimide structure, which reacts with modified cellulose, so that the furan group on the modified cellulose reacts with the maleimide structure to form a dynamic covalent bond. Through the multi-layer dynamic covalent bonds, the phenolic resin adhesive can dissipate a large amount of energy through the breaking and reorganization process of the dynamic covalent bonds after being impacted, thereby playing a role in buffering energy absorption and impact resistance, thereby enhancing the toughness of the phenolic resin adhesive. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] A method for preparing a colorless and transparent phenolic resin adhesive comprises the following steps:

[0023] Step A1: γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane and deionized water were mixed, stirred for 10 min at a speed of 200 r / min and a temperature of 60° C., concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane were added, reacted for 4 h, and the pH was adjusted to neutral to obtain intermediate 1;

[0024] Step A2: Tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and DMF are mixed evenly, stirred at a speed of 150 r / min and a temperature of 50° C., chloroplatinic acid is added, and the reaction is carried out for 6 hours, p-hydroxystyrene is added, and the reaction is continued for 8 hours to obtain intermediate 2, intermediate 2, 4-formylphenylboronic acid and DMF are mixed evenly, stirred at a speed of 120 r / min and a temperature of 45° C., sodium cyanoborohydride is added, and the reaction is carried out for 20 hours to obtain a modified monomer;

[0025] Step A3: Weigh the following raw materials in parts by weight: 60 parts of phenol, 30 parts of modified monomer, 180 parts of formaldehyde solution, 3 parts of sodium hydroxide solution and 5 parts of reinforcing filler, mix the phenol, modified monomer and sodium hydroxide solution evenly, stir for 20 minutes at a speed of 120 r / min and a temperature of 80°C, raise the temperature to 90°C, add the formaldehyde solution and reinforcing filler, and react for 1 hour to obtain a phenolic resin adhesive.

[0026] The amount ratio of γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane, deionized water and 1,1,3,3-tetramethyldisiloxane described in step A1 is 1mmol:2mmol:20mL:1.5mmol, and the amount of concentrated sulfuric acid is 2% of the mass of γ-aminopropylmethyldiethoxysilane.

[0027] The molar ratio of tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and p-hydroxystyrene described in step A2 is 1:4:4, the amount of chloroplatinic acid used is 1‰ of the mass of tetramethyltetravinylcyclotetrasiloxane, the molar ratio of the amino group on intermediate 2 and 4-formylphenylboric acid is 1:1, and the amount of sodium cyanoborohydride used is 3% of the mass of intermediate 2.

[0028] The mass fraction of the sodium hydroxide solution described in step A3 is 40%, and the mass fraction of the formaldehyde solution is 37%.

[0029] The reinforcing filler is prepared by the following steps:

[0030] Step B1: adding cellulose to a sodium hydroxide solution, reacting for 3 hours at a speed of 120 r / min and a temperature of 50° C., filtering the filtrate, washing to neutrality, and obtaining alkalized cellulose; uniformly mixing the alkalized cellulose, epichlorohydrin and dioxane, stirring and adding sodium hydroxide at a speed of 60 r / min and a temperature of 35° C., and reacting for 2 hours to obtain pretreated cellulose; uniformly mixing the pretreated cellulose, furfurylamine and DMF, and reacting for 3 hours at a speed of 120 r / min, a temperature of 30° C. and a pH value of 10 to obtain modified cellulose;

[0031] Step B2: Mix hexagonal boron nitride, urea and deionized water evenly, grind for 10-15 hours, filter and remove the filtrate, disperse the substrate in ethanol, add 3-isocyanatepropyltrimethoxysilane, react for 3 hours at a speed of 120r / min and a temperature of 40°C to obtain pretreated hexagonal boron nitride, dissolve maleic anhydride in toluene, stir and add 3-aminopropyltriethoxysilane at a speed of 150r / min and a temperature of 50°C, react for 1 hour, add sodium acetate and hydroquinone, heat to 110°C, and reflux for 2 hours to obtain a modifier;

[0032] Step B3: Disperse the pretreated hexagonal boron nitride in dimethyl sulfoxide, add a modifier, react for 10 hours at a speed of 120 r / min and a temperature of 60°C, cool to 20°C, add ammonium fluoride, and react for 20 hours to obtain modified hexagonal boron nitride. Mix the modified hexagonal boron nitride, modified cellulose and DMF, react for 8 hours at a speed of 200 r / min and a temperature of 20°C, filter and remove the filtrate and dry to obtain a reinforced filler.

[0033] The dosage ratio of cellulose and sodium hydroxide solution in step B1 is 1g:10mL, the mass fraction of sodium hydroxide solution is 4%, the dosage ratio of alkalized cellulose, epichlorohydrin and sodium hydroxide is 1g:25mL:5g, and the molar ratio of epoxy group and furfurylamine on pretreated cellulose is 1:1.

[0034] The amount ratio of hexagonal boron nitride, urea, deionized water and 3-isocyanatepropyltrimethoxysilane described in step B2 is 1g:30g:30mL:3mL, the molar ratio of maleic anhydride and 3-aminopropyltriethoxysilane is 1:1, the amount of sodium acetate is 5% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane, and the amount of hydroquinone is 0.7% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane.

[0035] The mass ratio of the pretreated hexagonal boron nitride, the modifier and the ammonium fluoride in step B3 is 2:2.5:0.3, and the mass ratio of the modified hexagonal boron nitride and the modified cellulose is 1:6.

[0036] Example 2

[0037] A method for preparing a colorless and transparent phenolic resin adhesive comprises the following steps:

[0038] Step A1: γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane and deionized water were mixed, stirred for 13 minutes at a speed of 200 r / min and a temperature of 65° C., concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane were added, reacted for 5 hours, and the pH was adjusted to neutral to obtain intermediate 1;

[0039] Step A2: Tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and DMF are mixed evenly, stirred at a speed of 150 r / min and a temperature of 55° C., chloroplatinic acid is added, and the reaction is carried out for 7 hours, p-hydroxystyrene is added, and the reaction is continued for 9 hours to obtain intermediate 2, intermediate 2, 4-formylphenylboronic acid and DMF are mixed evenly, stirred at a speed of 120 r / min and a temperature of 50° C., sodium cyanoborohydride is added, and the reaction is carried out for 23 hours to obtain a modified monomer;

[0040] Step A3: Weigh the following raw materials in parts by weight: 70 parts of phenol, 35 parts of modified monomer, 200 parts of formaldehyde solution, 4 parts of sodium hydroxide solution and 8 parts of reinforcing filler, mix the phenol, modified monomer and sodium hydroxide solution evenly, stir for 25 minutes at a speed of 120 r / min and a temperature of 85°C, raise the temperature to 95°C, add the formaldehyde solution and reinforcing filler, and react for 1.3 hours to obtain a phenolic resin adhesive.

[0041] The amount ratio of γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane, deionized water and 1,1,3,3-tetramethyldisiloxane described in step A1 is 1mmol:2mmol:20mL:1.5mmol, and the amount of concentrated sulfuric acid is 2% of the mass of γ-aminopropylmethyldiethoxysilane.

[0042] The molar ratio of tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and p-hydroxystyrene described in step A2 is 1:4:4, the amount of chloroplatinic acid used is 1‰ of the mass of tetramethyltetravinylcyclotetrasiloxane, the molar ratio of the amino group on intermediate 2 and 4-formylphenylboric acid is 1:1, and the amount of sodium cyanoborohydride used is 3% of the mass of intermediate 2.

[0043] The mass fraction of the sodium hydroxide solution described in step A3 is 40%, and the mass fraction of the formaldehyde solution is 37%.

[0044] The reinforcing filler is prepared by the following steps:

[0045] Step B1: adding cellulose to a sodium hydroxide solution, reacting for 4 hours at a speed of 150 r / min and a temperature of 53° C., filtering the filtrate, washing to neutrality, and obtaining alkalized cellulose; uniformly mixing the alkalized cellulose, epichlorohydrin and dioxane, stirring and adding sodium hydroxide at a speed of 60 r / min and a temperature of 38° C., and reacting for 3 hours to obtain pretreated cellulose; uniformly mixing the pretreated cellulose, furfurylamine and DMF, and reacting for 4 hours at a speed of 150 r / min, a temperature of 35° C. and a pH value of 10 to obtain modified cellulose;

[0046] Step B2: Mix hexagonal boron nitride, urea and deionized water evenly, grind for 15 hours, filter and remove the filtrate, disperse the substrate in ethanol, add 3-isocyanatepropyltrimethoxysilane, react for 4 hours at a speed of 120 r / min and a temperature of 45°C to obtain pretreated hexagonal boron nitride, dissolve maleic anhydride in toluene, stir and add 3-aminopropyltriethoxysilane at a speed of 150 r / min and a temperature of 55°C, react for 1.3 hours, add sodium acetate and hydroquinone, heat to 115°C, and reflux for 2.5 hours to obtain a modifier;

[0047] Step B3: Disperse the pretreated hexagonal boron nitride in dimethyl sulfoxide, add a modifier, react for 13 hours at a speed of 150 r / min and a temperature of 60°C, cool to 25°C, add ammonium fluoride, react for 23 hours to obtain modified hexagonal boron nitride, mix the modified hexagonal boron nitride, modified cellulose and DMF, react for 9 hours at a speed of 200 r / min and a temperature of 25°C, filter and remove the filtrate and dry to obtain a reinforced filler.

[0048] The dosage ratio of cellulose and sodium hydroxide solution in step B1 is 1g:10mL, the mass fraction of sodium hydroxide solution is 4%, the dosage ratio of alkalized cellulose, epichlorohydrin and sodium hydroxide is 1g:25mL:5g, and the molar ratio of epoxy group and furfurylamine on pretreated cellulose is 1:1.

[0049] The amount ratio of hexagonal boron nitride, urea, deionized water and 3-isocyanatepropyltrimethoxysilane described in step B2 is 1g:30g:30mL:3mL, the molar ratio of maleic anhydride and 3-aminopropyltriethoxysilane is 1:1, the amount of sodium acetate is 5% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane, and the amount of hydroquinone is 0.7% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane.

[0050] The mass ratio of the pretreated hexagonal boron nitride, the modifier and the ammonium fluoride in step B3 is 2:2.5:0.3, and the mass ratio of the modified hexagonal boron nitride and the modified cellulose is 1:6.

[0051] Example 3

[0052] A method for preparing a colorless and transparent phenolic resin adhesive comprises the following steps:

[0053] Step A1: γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane and deionized water were mixed, stirred for 15 min at a speed of 300 r / min and a temperature of 70° C., concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane were added, reacted for 6 h, and the pH was adjusted to neutral to obtain intermediate 1;

[0054] Step A2: Tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and DMF are mixed evenly, stirred at a speed of 200 r / min and a temperature of 60° C., chloroplatinic acid is added, and the reaction is carried out for 8 hours, p-hydroxystyrene is added, and the reaction is continued for 10 hours to obtain intermediate 2, intermediate 2, 4-formylphenylboronic acid and DMF are mixed evenly, stirred at a speed of 150 r / min and a temperature of 55° C., sodium cyanoborohydride is added, and the reaction is carried out for 25 hours to obtain a modified monomer;

[0055] Step A3: Weigh the following raw materials in parts by weight: 80 parts of phenol, 40 parts of modified monomer, 230 parts of formaldehyde solution, 5 parts of sodium hydroxide solution and 10 parts of reinforcing filler, mix the phenol, modified monomer and sodium hydroxide solution evenly, stir for 30 minutes at a speed of 150 r / min and a temperature of 85°C, raise the temperature to 95°C, add the formaldehyde solution and reinforcing filler, and react for 1.5 hours to obtain a phenolic resin adhesive.

[0056] The amount ratio of γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane, deionized water and 1,1,3,3-tetramethyldisiloxane described in step A1 is 1mmol:2mmol:20mL:1.5mmol, and the amount of concentrated sulfuric acid is 2% of the mass of γ-aminopropylmethyldiethoxysilane.

[0057] The molar ratio of tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and p-hydroxystyrene described in step A2 is 1:4:4, the amount of chloroplatinic acid used is 1‰ of the mass of tetramethyltetravinylcyclotetrasiloxane, the molar ratio of the amino group on intermediate 2 and 4-formylphenylboric acid is 1:1, and the amount of sodium cyanoborohydride used is 3% of the mass of intermediate 2.

[0058] The mass fraction of the sodium hydroxide solution described in step A3 is 40%, and the mass fraction of the formaldehyde solution is 37%.

[0059] The reinforcing filler is prepared by the following steps:

[0060] Step B1: adding cellulose to a sodium hydroxide solution, reacting for 5 hours at a speed of 150 r / min and a temperature of 55° C., filtering the filtrate, washing to neutrality, and obtaining alkalized cellulose; uniformly mixing the alkalized cellulose, epichlorohydrin and dioxane, stirring and adding sodium hydroxide at a speed of 80 r / min and a temperature of 40° C., and reacting for 4 hours to obtain pretreated cellulose; uniformly mixing the pretreated cellulose, furfurylamine and DMF, and reacting for 5 hours at a speed of 150 r / min, a temperature of 40° C. and a pH value of 11 to obtain modified cellulose;

[0061] Step B2: Hexagonal boron nitride, urea and deionized water are mixed evenly, ground for 15 hours, filtered to remove the filtrate, the substrate is dispersed in ethanol, 3-isocyanate propyltrimethoxysilane is added, and the reaction is carried out for 5 hours at a speed of 150 r / min and a temperature of 50°C to obtain pretreated hexagonal boron nitride, maleic anhydride is dissolved in toluene, and 3-aminopropyltriethoxysilane is added under stirring at a speed of 200 r / min and a temperature of 55°C. After reacting for 1.5 hours, sodium acetate and hydroquinone are added, the temperature is raised to 115°C, and refluxed for 3 hours to obtain a modifier;

[0062] Step B3: Disperse the pretreated hexagonal boron nitride in dimethyl sulfoxide, add a modifier, react for 15 hours at a speed of 150 r / min and a temperature of 65°C, cool to 25°C, add ammonium fluoride, and react for 25 hours to obtain modified hexagonal boron nitride. Mix the modified hexagonal boron nitride, modified cellulose and DMF, react for 10 hours at a speed of 300 r / min and a temperature of 25°C, filter and remove the filtrate and dry to obtain a reinforced filler.

[0063] The dosage ratio of cellulose and sodium hydroxide solution in step B1 is 1g:10mL, the mass fraction of sodium hydroxide solution is 4%, the dosage ratio of alkalized cellulose, epichlorohydrin and sodium hydroxide is 1g:25mL:5g, and the molar ratio of epoxy group and furfurylamine on pretreated cellulose is 1:1.

[0064] The amount ratio of hexagonal boron nitride, urea, deionized water and 3-isocyanatepropyltrimethoxysilane described in step B2 is 1g:30g:30mL:3mL, the molar ratio of maleic anhydride and 3-aminopropyltriethoxysilane is 1:1, the amount of sodium acetate is 5% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane, and the amount of hydroquinone is 0.7% of the total mass of maleic anhydride and 3-aminopropyltriethoxysilane.

[0065] The mass ratio of the pretreated hexagonal boron nitride, the modifier and the ammonium fluoride in step B3 is 2:2.5:0.3, and the mass ratio of the modified hexagonal boron nitride and the modified cellulose is 1:6.

[0066] Comparative Example 1

[0067] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.

[0068] Comparative Example 2

[0069] Compared with Example 1, this comparative example uses cellulose instead of the reinforcing filler, and the other steps are the same.

[0070] Comparative Example 3

[0071] Compared with Example 1, this comparative example uses hexagonal boron nitride to replace the reinforcing filler, and the other steps are the same.

[0072] Comparative Example 4

[0073] Compared with Example 1, in this comparative example, pretreated hexagonal boron nitride is dispersed in dimethyl sulfoxide, propyltriethoxysilane is added, and the reaction is carried out for 10 hours at a rotation speed of 120 r / min and a temperature of 60°C. The temperature is lowered to 20°C, ammonium fluoride is added, and the reaction is carried out for 20 hours. The obtained product replaces the reinforcing filler, and the remaining steps are the same.

[0074] The phenolic resin adhesives prepared in Examples 1-3 and Comparative Examples 1-4 were made into samples with a size of 80 mm×10 mm×10 mm, and V-notches with a depth of 2 mm were opened to test the impact strength according to the standard of GB / T1043-1993.

[0075]

[0076] It can be seen from the above table that this application has a good impact resistance effect.

[0077] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a colorless and transparent phenolic resin adhesive, characterized in that: The specific steps include: Step A1: After mixing and stirring γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane and deionized water, concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added, and after reacting, the pH is adjusted to neutral to obtain an intermediate 1; Step A2: tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and DMF are mixed and stirred, and chloroplatinic acid is added to react, and p-hydroxystyrene is added to continue the reaction to obtain intermediate 2, and intermediate 2, 4-formylphenylboronic acid and DMF are mixed and stirred, and sodium cyanoborohydride is added to react to obtain a modified monomer; Step A3: weighing the following raw materials in parts by weight: 60-80 parts of phenol, 30-40 parts of modified monomer, 180-230 parts of formaldehyde solution, 3-5 parts of sodium hydroxide solution and 5-10 parts of reinforcing filler, mixing the phenol, modified monomer and sodium hydroxide solution, heating and adding the formaldehyde solution and reinforcing filler to react, and preparing a phenolic resin adhesive; The reinforcing filler is prepared by the following steps: Step B1: adding cellulose to a sodium hydroxide solution for reaction, filtering out the filtrate, washing to neutrality to obtain alkalized cellulose, mixing the alkalized cellulose, epichlorohydrin and dioxane, adding sodium hydroxide for reaction to obtain pretreated cellulose, and mixing the pretreated cellulose, furfurylamine and DMF for reaction to obtain modified cellulose; Step B2: Mix and grind hexagonal boron nitride, urea and deionized water, filter and remove the filtrate, disperse the substrate in ethanol, add 3-isocyanatepropyltrimethoxysilane, react to obtain pretreated hexagonal boron nitride, dissolve maleic anhydride in toluene, stir and add 3-aminopropyltriethoxysilane, react, add sodium acetate and hydroquinone, heat and reflux to obtain a modifier; Step B3: Disperse the pretreated hexagonal boron nitride in dimethyl sulfoxide, add a modifier, react, add ammonium fluoride, continue the reaction to obtain modified hexagonal boron nitride, mix the modified hexagonal boron nitride, modified cellulose and DMF for reaction, filter to remove the filtrate and dry to obtain a reinforcing filler.

2. The method for preparing a colorless and transparent phenolic resin adhesive according to claim 1, characterized in that: The amount ratio of γ-aminopropylmethyldiethoxysilane, diphenyldichlorosilane, deionized water and 1,1,3,3-tetramethyldisiloxane described in step A1 is 1 mmol:2 mmol:20 mL:1.5 mmol.

3. The method for preparing a colorless and transparent phenolic resin adhesive according to claim 1, characterized in that: The molar ratio of tetramethyltetravinylcyclotetrasiloxane, intermediate 1 and p-hydroxystyrene described in step A2 is 1:4:4, and the molar ratio of the amino group on intermediate 2 and 4-formylphenylboronic acid is 1:

1.

4. The method for preparing a colorless and transparent phenolic resin adhesive according to claim 1, characterized in that: The mass fraction of the sodium hydroxide solution described in step A3 is 40%, and the mass fraction of the formaldehyde solution is 37%.

5. The method for preparing a colorless and transparent phenolic resin adhesive according to claim 1, characterized in that: The dosage ratio of cellulose and sodium hydroxide solution in step B1 is 1g:10mL, the mass fraction of sodium hydroxide solution is 4%, the dosage ratio of alkalized cellulose, epichlorohydrin and sodium hydroxide is 1g:25mL:5g, and the molar ratio of epoxy group and furfurylamine on pretreated cellulose is 1:

1.

6. The method for preparing a colorless and transparent phenolic resin adhesive according to claim 1, characterized in that: The amount ratio of hexagonal boron nitride, urea, deionized water and 3-isocyanatepropyltrimethoxysilane described in step B2 is 1g:30g:30mL:3mL, and the molar ratio of maleic anhydride and 3-aminopropyltriethoxysilane is 1:

1.

7. The method for preparing a colorless and transparent phenolic resin adhesive according to claim 1, characterized in that: The mass ratio of the pretreated hexagonal boron nitride, the modifier and the ammonium fluoride in step B3 is 2:2.5:0.3, and the mass ratio of the modified hexagonal boron nitride and the modified cellulose is 1:

6.

8. A colorless and transparent phenolic resin adhesive, characterized in that: Prepared according to any one of claims 1 to 7.