Windshield organic silica gel and preparation method thereof
Through the combination of hydrogen-terminated phenyl polysiloxane and hydroxy-terminated polymethylphenyl siloxane and the use of modified ethylene-vinyl acetate copolymers, a three-dimensional network structure is formed, which solves the wind barrier in front of low-speed electric vehicles The initial test of glass organic silicone is insufficient in viscosity and tensile strength, which achieves higher bonding performance and operating feasibility.
Patent Information
- Application Number
- CN202410312398.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-03-19
AI Technical Summary
The prior art is difficult to effectively improve the initial test viscosity and tensile strength of silicone in front windshield of low-speed electric vehicles, especially in the application of glass materials, which fail to solve the initial test viscosity and strength problems at the same time.
Combination of hydrogen-terminated phenyl polysiloxane and hydroxy-terminated polymethylphenyl siloxane is adopted, and a modified ethylene-vinyl acetate copolymer is added, and the action of diisopropyl benzene peroxide catalyst is carried out with 3- (acryloyloxy)propyltrimethoxysilane is modified to form a three-dimensional network structure to improve the bonding strength and adhesion of silicone.
Significantly improve the initial viscosity and tensile strength of the silicone, avoid the windshield slipping during operation, enhance the feasibility of the application operation process, and show higher adhesion, toughness and mechanics in practical applications. strength.
Smart Images

Figure BDA0004747924960000111 
Figure BDA0004747924960000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives containing polymer compounds, and in particular to windshield organic silica gel and a preparation method thereof. Background Art
[0002] Silicone sealant is a sealing material made of silicone rubber as the base material by adding a certain proportion of additives and fillers. Silicone rubber is a polymer compound made of silicone compounds. When used as a sealant in the front windshield of low-speed electric vehicles, it usually needs to have properties such as sealing, UV resistance, shock resistance, and adhesion. Good sealing performance can effectively prevent water vapor, wind, sand and noise from entering the interior of the vehicle, fill and seal the gap between the windshield and the body, and ensure the sealing and comfort of the interior environment; the UV resistance of silicone rubber extends the service life of the windshield by preventing UV damage, and reduces the aging and fading of internal materials; the elasticity and shock resistance of silicone rubber can absorb and alleviate the impact and vibration of the windshield, improve the vehicle's shock resistance, and reduce the risk of windshield breakage; good adhesion performance can firmly adhere to the windshield and the body, and is not easy to fall off or deform, ensuring the stability and safety of the windshield.
[0003] In order to improve the performance of organic silica gel as a sealant on the front windshield of the car in the prior art, for example, the strength of organic silica gel can be significantly improved by selecting a suitable filler. Common fillers such as silica, carbon black, etc. can increase the mechanical strength of silica gel and improve its wear resistance; by optimizing the ratio of the cross-linking agent, the cross-linking degree of silica gel and the density of the network structure can be controlled, thereby affecting its adhesion and strength. The cross-linking agent is a key component in the formation of the network structure in organic silica gel. Properly increasing the content of the cross-linking agent may also improve the strength of the silica gel, but too much cross-linking agent may cause the silica gel to harden too much and reduce its viscosity; select a suitable catalyst. The catalyst plays a key role in the cross-linking reaction of organic silica gel. Selecting a suitable catalyst can increase the cross-linking rate and degree of cross-linking, thereby improving the adhesion and strength of the silica gel; functional enhancers can also be added to improve the adhesion and strength of organic silica gel, such as fiber materials, nanoparticles, etc., which can form a reinforced network in silica gel to provide additional mechanical strength. With the development of technology, organic silica gel has been improved to varying degrees in various performances to meet the higher requirements of low-speed electric vehicles for windshields.
[0004] CN105419722A discloses a method for preparing a silicone sealant for bonding automobile headlights and fog lamps. The sealant is composed of a base material, silicone oil, an inhibitor, a catalyst, a tackifier, and a reinforcing filler. The base material is dihydroxy polydimethylsiloxane, a hydrogen-containing alkoxysilane end-capping agent, an alkoxysilane cross-linking agent, and anilinomethyl triethoxysilane. The silicone sealant for bonding automobile headlights and fog lamps obtained by the preparation method of the invention is a single-component neutral cure, has no corrosive effect on materials, has a long service life, is easy to extrude, but does not flow, is easy to operate, can be applied manually or mechanically, and can meet any working environment and working conditions; the invention has excellent bonding strength, has good bonding properties and high bonding strength to various plastics such as ABS, PVC, high-density polystyrene (HIPS), microcrystalline glass and metal, and generally does not require the use of a primer.
[0005] CN114574153A discloses an organic silicone sealant and a preparation method thereof, wherein the organic silicone sealant is composed of the following components: 80-120 parts of vinyl silicone oil; 1-5 parts of fumed silica; 0.5-10 parts of hydrogen-containing silicone oil; 0.1-0.5 parts of platinum catalyst; 1-5 parts of tackifier; 200-300 parts of thermal conductive filler; 0.01-0.05 parts of organic titanium catalyst. The invention uses terminal hydrogen-containing polysiloxane for chain extension and crosslinking, and adopts a special tackifier compound, which has the addition type silicone rubber self-adhesive technology and improves the substrate bonding applicability; the single-component addition type silicone rubber product of the invention has stable storage, low curing temperature and short curing time, self-adhesiveness, is suitable for stainless steel, aluminum alloy, PC and other materials, and has low compression permanent deformation.
[0006] The above invention patents all add tackifiers to improve the adhesion of silicone sealing silica gel, but do not more specifically solve the initial adhesion of silicone sealant before curing and its application on glass materials, nor do they solve the initial adhesion and strength problems at the same time. Summary of the invention
[0007] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to improve the initial adhesion and tensile strength of the organic silicone used for the front windshield of a low-speed electric vehicle.
[0008] To achieve the above object, the present invention provides a windshield organic silica gel and a preparation method thereof.
[0009] Specifically, the preparation method of the windshield organic silica gel comprises the following steps, measured in parts by weight:
[0010] First, 30-40 parts of polysiloxane and 60-80 parts of filler are mixed, and then 2-4 parts of dimethyl silicone oil, 0.01-0.05 parts of titanate, and 2-6 parts of vinyl trisbutyl ketoxime silane are added, and stirring is continued for 1-2 hours under the conditions of 0.06-0.08MPa vacuum degree and 60°C-100°C. After cooling to room temperature, 0.1-2 parts of tackifier are added, and stirring is carried out at room temperature for 0.5-1 hour. Finally, the mixture is filled into a sealed container to obtain the windshield organic silica gel.
[0011] The polysiloxane is any one of hydrogen-terminated phenyl polysiloxane and hydroxyl-terminated polymethylphenyl siloxane or a mixture of the two; preferably, hydrogen-terminated phenyl polysiloxane and hydroxyl-terminated polymethylphenyl siloxane are mixed in a ratio of 1-2:0.1-0.5.
[0012] The titanate is produced by Dovkaite ET, TPT, 726, 722, Any one or a mixture of OGT.
[0013] The filler is any one of fumed white carbon black, alumina, nano calcium carbonate, silicon carbide and kaolin, or a mixture thereof.
[0014] The tackifier is any one of ethylene-vinyl acetate copolymer and modified ethylene-vinyl acetate copolymer or a mixture thereof.
[0015] The modification method of the modified ethylene-vinyl acetate copolymer is as follows, in parts by weight:
[0016] 0.01-0.02 parts of diisopropylbenzene peroxide and 0.01-0.04 parts of 3-(acryloyloxy)propyltrimethoxysilane are added to 1-2 parts of ethylene-vinyl acetate copolymer and stirred at room temperature for 0.5-1 hour, stirred at 150-170°C and 80-100r / min for 10-30min, cooled to room temperature, added to 20-40 parts of xylene, stirred at 40-60°C for 1-2 hours to obtain a mixed solution, and dropped into 20-40 parts of methanol at room temperature while hot, stirred while precipitating, filtered, and dried the filter cake at 40-60°C to obtain a modified ethylene-vinyl acetate copolymer.
[0017] Polysiloxane is the main component of organic silica gel. In the present invention, polysiloxane is a compound of hydrogen-terminated phenyl polysiloxane and hydroxyl-terminated polymethylphenyl siloxane. Hydrogen-terminated phenyl polysiloxane can provide higher bonding strength. Hydroxyl-terminated polymethylphenyl siloxane has good adhesion, heat resistance and weather resistance, and can still maintain stability at high temperatures. Its hydroxyl-terminated can participate in the cross-linking reaction during the curing process, which helps to form a three-dimensional network structure of silica gel and improve the strength and durability of silica gel. The compound of the two can be convenient for fixing the front windshield when the glue is not yet cured, keeping the two surfaces bonded together and not slipping during operation. The filler added in the organic silica gel plays a role in increasing the volume of the material and adjusting the rheological properties of silica gel. A small amount of dimethyl silicone oil is added to help lubricate and improve processability. The titanate cross-linking agent can make the silica gel form a three-dimensional network structure during the curing process, increase the strength and durability of the silica gel, and the vinyl trisbutyl ketoxime silane promotes the cross-linking reaction during the curing process of the silica gel, thereby improving the bonding strength and adhesion of the silica gel. Ethylene-vinyl acetate copolymer has good flexibility, elasticity, biocompatibility and low permeability. It is modified with 3-(acryloyloxy)propyltrimethoxysilane under the action of diisopropyl peroxide catalyst. The introduction of polar groups in 3-(acryloyloxy)propyltrimethoxysilane enhances the van der Waals force and the number of polar sites between molecular chains, increases its cohesive strength, and is found to have improved initial adhesion. In practical applications, it can prevent the windshield from slipping during operation before fixation, thereby enhancing the feasibility of the application operation process. It may also exhibit higher adhesion, toughness and mechanical strength, making it more suitable for bonding windshield surfaces, and exhibiting higher strength and durability.
[0018] Beneficial effects of the present invention:
[0019] Compared with the prior art, the windshield organic silica gel of the present invention is compounded with hydrogen-terminated phenyl polysiloxane and hydroxyl-terminated polymethylphenyl siloxane, and the compounding of the two can facilitate the fixing of the front windshield when the glue is not yet solidified, keep the two surfaces bonded together, and will not slip during operation. Modified ethylene-vinyl acetate copolymer is also added, and modified with 3-(acryloyloxy)propyltrimethoxysilane under the action of diisopropylbenzene peroxide catalyst. The introduction of polar groups in 3-(acryloyloxy)propyltrimethoxysilane enhances the van der Waals force and the number of polar sites between molecular chains, increases its cohesive strength, and finds that its initial adhesion is improved, which prevents the windshield from slipping during operation before fixing in practical applications, and enhances the feasibility of the application operation process. DETAILED DESCRIPTION
[0020] The parameters of the specific chemical substances used in the examples are from the following sources:
[0021] Ethylene-vinyl acetate copolymer: purity 98wt%, industrial grade, manufacturer is Henan Weitixi Chemical Technology Co., Ltd., item number is A0937788.
[0022] Vinyl trisbutyl ketone oxime silane: The manufacturer is Hubei Shiteng Chemical Technology Co., Ltd., the product number is 032563.
[0023] Hydrogen-terminated phenyl polysiloxane: The active ingredient content is 99wt%, the manufacturer is Chongqing Ruiya Biotechnology Co., Ltd., and the product number is 68952-30-7.
[0024] Hydroxyl-terminated polymethylphenylsiloxane: the active ingredient content is 99wt%, the manufacturer is Hubei Jusheng Technology Co., Ltd., and the product number is JS8084.
[0025] Fumed silica: Specific surface area is 200m 2 / g, the silicon dioxide content is 99.8%, the manufacturer is Anhui Aiyota Silicone Oil Co., Ltd., and the model is HL4200.
[0026] Example 1
[0027] A method for preparing windshield organic silica gel comprises the following steps:
[0028] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum degree and 80°C, cool to room temperature, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0029] Example 2
[0030] A method for preparing windshield organic silica gel comprises the following steps:
[0031] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0032] Example 3
[0033] A method for preparing windshield organic silica gel comprises the following steps:
[0034] First, 360g hydrogen-terminated phenyl polysiloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0035] Example 4
[0036] A method for preparing windshield organic silica gel comprises the following steps:
[0037] First, 343g hydrogen-terminated phenyl polysiloxane, 17g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0038] Example 5
[0039] A method for preparing windshield organic silica gel comprises the following steps:
[0040] First, 277g hydrogen-terminated phenyl polysiloxane, 83g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0041] Example 6
[0042] A method for preparing windshield organic silica gel comprises the following steps:
[0043] First, 180g hydrogen-terminated phenyl polysiloxane, 180g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0044] Example 7
[0045] A method for preparing windshield organic silica gel comprises the following steps:
[0046] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of modified ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0047] The modification method of the modified ethylene-vinyl acetate copolymer is as follows:
[0048] Add 0.15 g of diisopropyl peroxide and 0.25 g of 3-(acryloyloxy)propyltrimethoxysilane to 18 g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5 hour, stir at 150°C and 80 r / min for 20 minutes, cool to room temperature, add to 400 g of xylene, stir at 45°C for 1.5 hours to obtain a mixed solution, dropwise add into 400 g of methanol at room temperature while hot, stir while precipitating, filter and dry the filter cake at 45°C to obtain a modified ethylene-vinyl acetate copolymer.
[0049] Comparative Example 1
[0050] A method for preparing windshield organic silica gel comprises the following steps:
[0051] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of modified ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0052] The modification method of the modified ethylene-vinyl acetate copolymer is as follows:
[0053] Add 0.15g of diisopropylbenzene peroxide and 0.25g of vinylmethyldiethoxysilane to 18g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5 hour, stir at 150°C and 80r / min for 20min, cool to room temperature, add to 400g of xylene, stir at 45°C for 1.5 hours to obtain a mixed solution, dropwise add into 400g of methanol at room temperature while hot, stir while precipitating, filter and dry the filter cake at 45°C to obtain a modified ethylene-vinyl acetate copolymer.
[0054] Comparative Example 2
[0055] A method for preparing windshield organic silica gel comprises the following steps:
[0056] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of modified ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0057] The modification method of the modified ethylene-vinyl acetate copolymer is as follows:
[0058] Add 0.15g of diisopropyl peroxide and 0.25g of γ-methacryloxypropyltrimethoxysilane to 18g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5 hour, stir at 150°C and 80r / min for 20min, cool to room temperature, add to 400g of xylene, stir at 45°C for 1.5 hours to obtain a mixed solution, dropwise add into 400g of methanol at room temperature while hot, stir while precipitating, filter and dry the filter cake at 45°C to obtain a modified ethylene-vinyl acetate copolymer.
[0059] Comparative Example 3
[0060] A method for preparing windshield organic silica gel comprises the following steps:
[0061] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of modified ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0062] The modification method of the modified ethylene-vinyl acetate copolymer is as follows:
[0063] Add 0.15g of diisopropylbenzene peroxide and 0.25g of vinyl tri(2-methoxyethoxy)silane to 18g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5 hour, stir at 150°C and 80r / min for 20min, cool to room temperature, add to 400g of xylene, stir at 45°C for 1.5 hours to obtain a mixed solution, dropwise add into 400g of methanol at room temperature while hot, stir while precipitating, filter and dry the filter cake at 45°C to obtain a modified ethylene-vinyl acetate copolymer.
[0064] Comparative Example 4
[0065] A method for preparing windshield organic silica gel comprises the following steps:
[0066] First, 300g hydrogen-terminated phenyl polysiloxane, 60g hydroxyl-terminated polymethylphenyl siloxane, 100g fumed silica, 150g 1000 mesh silicon carbide, and 400g 1250 mesh kaolin were mixed, and then 35g dimethyl silicone oil and 0.3g TPT titanate, 40g of vinyl trisbutyl ketoxime silane, continue stirring for 1.5h under the conditions of 0.08MPa vacuum and 80°C, cool to room temperature, add 15g of modified ethylene-vinyl acetate copolymer, stir at room temperature for 0.5h, and finally fill into a sealed container to obtain the windshield organic silica gel.
[0067] The modification method of the modified ethylene-vinyl acetate copolymer is as follows:
[0068] Add 0.15g of diisopropylbenzene peroxide and 0.25g of diethylaminomethyltriethoxysilane to 18g of ethylene-vinyl acetate copolymer, stir at room temperature for 0.5 hour, stir at 150°C and 80r / min for 20min, cool to room temperature, add to 400g of xylene, stir at 45°C for 1.5 hours to obtain a mixed solution, dropwise add into 400g of methanol at room temperature while hot, stir while precipitating, filter and dry the filter cake at 45°C to obtain a modified ethylene-vinyl acetate copolymer.
[0069] Test Example 1
[0070] Tensile Adhesion Test
[0071] The windshield organic silica gel obtained by the preparation method of Examples 1-7 and Comparative Examples 1-4 was bonded between the surfaces of two parallel substrates to prepare a test piece, the substrate being a glass plate of 50 mm×50 mm×12 mm; the test piece was stretched to failure, and the tensile bonding performance of the sealing material was expressed by calculating the maximum tensile strength. The test procedure was based on the national standard GB / T 13477.8-2017 "Test methods for building sealing materials Part 8: Determination of tensile bonding properties", and the test treatment was based on method A. The prepared test piece was placed under standard test conditions for 28 days, and an initial adhesion test was added, that is, the prepared test piece was tested immediately.
[0072] Preparation of test specimens: Use degreased gauze to remove dust from the surface of cement mortar board, use ethanol and water to clean glass plate, and dry; keep it at 23°C, use organic silica gel to adhere substrate to prepare test specimen, assemble two adhesive substrates and two isolation pads on anti-adhesive material to form a cavity; then embed the windshield organic silica gel sample obtained by the preparation method of Examples 1-7 and Comparative Examples 1-4 in the cavity, and make test specimens after surface drying, and prepare 3 test specimens for each group of tests; pay attention to the following matters when embedding the sample: a) avoid forming bubbles; b) squeeze the sample on the adhesive surface of the substrate to make it tightly bonded; c) trim the surface of the sample to make it flush with the upper surface of the substrate and the pad. The isolation pad: the surface should be anti-adhesive, used to prepare the test specimen with a sealing material cross-section of 12mm×12mm; the anti-adhesive material: anti-adhesive film or anti-adhesive paper, such as polyethylene (PE) film, etc.
[0073] Test steps: Place the specimen on its side and remove the anti-sticking material as soon as possible to allow the specimen to fully cure or dry completely; during the curing period, the isolation pad should be kept in place; when the selected substrate size may affect the curing speed of the specimen, the isolation pad should be separated from the sealing material as soon as possible, but it still needs to be kept in place; remove the isolation pad on the specimen, load the specimen into the tensile testing machine, stretch the specimen to failure at a speed of 5.5mm / min at 23°C, and record the force-elongation curve and failure form.
[0074] The maximum tensile strength (T s ) is calculated according to the following formula and the arithmetic mean of the three specimens is taken, accurate to 0.01MPa.
[0075] T s =P / S
[0076] Where:
[0077] T s——maximum tensile strength, in megapascals (MPa);
[0078] P——maximum tension value, in Newton (N);
[0079] S——The initial cross-sectional area of the specimen, in square millimeters (mm 2 ).
[0080] Table 1 Tensile Adhesion Test Data
[0081]
[0082] In Test Example 1, the maximum tensile strength of initial adhesion is tested immediately after the sample is prepared, and it is not placed under standard test conditions for 28 days. The tensile strength refers to the maximum tensile force that the material can withstand before breaking in the tensile test. The higher the tensile strength of the organic silicone, the better its tensile adhesion and durability. From the comparison of Test Example 1, it can be seen that the difference between Examples 1-2 lies in whether ethylene-vinyl acetate copolymer is added. It is found that the addition of ethylene-vinyl acetate copolymer can enhance the tensile strength, but has no effect on the maximum tensile strength of initial adhesion; in Examples 2-6, polysiloxanes are compounded in different proportions, and it is found that the windshield organic silicone obtained by the preparation method of Example 2 has the highest maximum tensile strength both in initial adhesion and after 28 days of placement. In Example 7, ethylene-vinyl acetate copolymer is modified on the basis of Example 2, and 4 groups of comparative examples are set up. The difference between Example 7 and Comparative Examples 1-4 is that different silanes are used in the modification method. Tests show that both Example 7 and Comparative Examples 1-4 have a certain improvement in initial adhesion, among which Example 7 has the best effect, and the maximum tensile strength of initial adhesion is 2.2 MPa. In actual application, the windshield before fixation can be prevented from slipping during operation, thereby enhancing the feasibility of the application operation process.
[0083] Test Example 2
[0084] Shear strength test
[0085] The windshield silicone rubber obtained by the preparation methods of Examples 1-7 and Comparative Examples 1-4 was applied to the glass surface and bonded in the shape specified in the test standard. The bonding surface length was 12.5 mm, the adhesive layer thickness was 0.1 mm, and the main axis direction of the sample should be consistent with the cutting direction of the silicone rubber at the bonding point. The test procedure was based on the national standard GB / T 7124-2008 "Determination of tensile shear strength of adhesives (rigid material to rigid material)" to test the shear strength of the glass.
[0086] Clamp the sample symmetrically on the fixture, with the distance from the clamp to the nearest bonding end being 50mm. A gasket can be used in the fixture to ensure that the force is within the bonding surface. The tensile testing machine is tested at a constant test speed so that the general failure time is between 65s±20s. If the tensile testing machine can load at a constant rate, set the shear force change rate between 8.3-9.8MPa per minute. Record the maximum load of the sample shear failure as the failure load.
[0087] Tensile shear strength (MPa) = breaking load (N) / shear area (mm), the test data is taken as the average value.
[0088] Table 2 Shear strength test data
[0089]
[0090] The tensile shear strength refers to the shear stress at the single lap joint of the glass material calculated by applying a tensile force parallel to the bonding surface and in the direction of the main axis of the sample. The greater the shear stress, the better the adhesion. From the comparison of Test Example 2, it can be seen that the shear strength of Example 7 is the largest, indicating that the windshield organic silicone obtained by the preparation method of the present invention has good bonding performance to glass.
Claims
1. A method for preparing windshield organic silica gel, characterized in that: The method comprises the following steps, in parts by weight: First, 30-40 parts of polysiloxane and 60-80 parts of filler are mixed, and then 2-4 parts of dimethyl silicone oil, 0.01-0.05 parts of titanate, and 2-6 parts of vinyl trisbutyl ketoxime silane are added, and stirring is continued for 1-2 hours under the conditions of 0.06-0.08MPa vacuum degree and 60°C-100°C, and then cooled to room temperature, 0.1-2 parts of tackifier are added, and stirred at room temperature for 0.5-1 hour, and finally filled into a sealed container to obtain the windshield organic silica gel; The tackifier is any one of ethylene-vinyl acetate copolymer and modified ethylene-vinyl acetate copolymer or a mixture thereof; The modification method of the modified ethylene-vinyl acetate copolymer is as follows, in parts by weight: 0.01-0.02 parts of diisopropylbenzene peroxide and 0.01-0.04 parts of 3-(acryloyloxy)propyltrimethoxysilane are added to 1-2 parts of ethylene-vinyl acetate copolymer and stirred at room temperature for 0.5-1 hour, stirred at 150-170° C. and 80-100 r / min for 10-30 minutes, cooled to room temperature, added to 20-40 parts of xylene, stirred at 40-60° C. for 1-2 hours to obtain a mixed solution, and dripped into 20-40 parts of methanol at room temperature while hot, stirred while precipitating, filtered, and dried the filter cake at 40-60° C. to obtain a modified ethylene-vinyl acetate copolymer; The polysiloxane is a mixture of hydrogen-terminated phenyl polysiloxane and hydroxyl-terminated polymethylphenyl siloxane in a ratio of 1-2:0.1-0.
5.
2. The method for preparing windshield organic silica gel according to claim 1, characterized in that: The titanate is any one of Tyzor® ET, Tyzor® TPT, Tyzor® 726, Tyzor® 722 and Tyzor® OGT produced by Dovkaite Corporation or a mixture thereof.
3. The method for preparing windshield organic silica gel according to claim 1, characterized in that: The filler is any one of fumed white carbon black, alumina, nano calcium carbonate, silicon carbide and kaolin, or a mixture thereof.
4. A windshield organic silica gel, characterized in that: The method is prepared by any one of claims 1 to 3.