One-dimensional Pt-based nanowire catalyst supported by nitride hollow nanotubes and preparation method thereof

By loading the Pt-based nanowire catalyst on the hollow nitride nanotube, the cost and stability of the platinum-based catalyst is solved, and a high-activity and low-cost catalyst is achieved. It is suitable for industrial applications of hydrogen fuel cells and significantly improves oxygen Electrochemical properties of reduction reactions.

CN118099452BActive Publication Date: 2024-11-15HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410053202.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2024-11-15
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

The life and cost issues of platinum-based catalysts are the main bottlenecks that restrict the large-scale application of hydrogen fuel cells. There are no mature cases in the prior art in improving the production cost of catalysts and component stability.

Method used

One-dimensional Pt-based nanowire catalyst based on nitride hollow nanotube loading was prepared by solvothermal method and oil bath heating method. The Pt-based nanowire was loaded to the surface of nitride hollow nanotube by liquid phase method and annealed under a specific atmosphere. Form a one-dimensional Pt-based nanowire catalyst with high activity and high stability.

Benefits of technology

The unit mass platinum activity of this catalyst is 2 to 10 times that of commercial Pt/C catalysts, and has extremely high stability and low cost. It is suitable for the industrial application of proton exchange membrane fuel cells, significantly improving the electrochemical performance of oxygen reduction reactions .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118099452B_ABST
    Figure CN118099452B_ABST
Patent Text Reader

Abstract

The present invention provides a one-dimensional Pt-based nanowire catalyst based on nitride hollow nanotube loading and a preparation method thereof. First, titanium oxide nanotubes are prepared by a solvothermal method, and nitride hollow nanotubes are obtained by nitridation treatment; one-dimensional Pt-based nanowires are obtained by an oil bath heating method; and then the Pt-based nanowires are loaded onto the surface of the nitride hollow nanotubes by a liquid phase method, and annealed in an Ar / H2 atmosphere to obtain a one-dimensional Pt-based nanowire catalyst based on nitride. The catalyst can be used as a cathode catalyst for a low-temperature fuel cell, and an effective combination of a high-performance one-dimensional structure and a high-stability hollow structure is achieved while reducing the amount of precious metals used in the fuel cell. The preparation method is simple to operate, has a stable structure, is suitable for large-scale industrial production and processing, and has important research significance for promoting the commercialization of high-performance low-platinum catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fuel cells, and in particular to a one-dimensional Pt-based nanowire catalyst supported by nitride hollow nanotubes and a preparation method thereof. Background Art

[0002] Hydrogen fuel cells are regarded as a kind of energy converter for hydrogen energy. They have the characteristics of fast hydrogen charging speed and pollution-free emission, and have been favored by researchers from various countries. As one of the power sources of automobiles, hydrogen fuel cells are not limited by the thermal efficiency of the Carnot cycle, and the energy conversion efficiency can easily exceed 60%. If they continue to develop in the long run, they will definitely become one of the directions for the sustainable development of the future automobile industry. Therefore, governments of various countries strongly support the development and use of hydrogen fuel vehicles, and provide considerable tax exemptions, purchase subsidies and other incentives. However, the life and cost of platinum-based catalysts are the main bottlenecks restricting the large-scale application of hydrogen fuel cells.

[0003] At present, the development and utilization of core technologies such as proton exchange membranes and reaction catalysts in China have made great progress. However, in terms of realizing the industrialization and marketization of automobiles, there are still no mature cases to refer to in terms of production costs and component stability. Various technical and performance improvement issues need to be urgently addressed. Summary of the invention

[0004] In view of this, the present invention proposes a one-dimensional Pt-based nanowire catalyst supported by nitride hollow nanotubes and a preparation method thereof to solve the above problems. The method has better performance than commercial Pt / C catalysts and reduces the loading of precious metal catalysts, reducing the cost of oxygen reduction catalysts, which is of great significance to promoting the commercialization of oxygen reduction catalysts.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] The present invention provides a method for preparing a one-dimensional Pt-based nanowire catalyst supported by nitride hollow nanotubes, comprising:

[0007] 1) Titanium oxide nanotubes are prepared by a solvothermal method, and nitride hollow nanotubes are obtained by nitridation treatment; one-dimensional Pt-based nanowires are obtained by an oil bath heating method;

[0008] 2) Pt-based nanowires were loaded onto the surface of nitride hollow nanotubes by a liquid phase method, and annealed in an Ar / H2 atmosphere to obtain a one-dimensional Pt-based nanowire catalyst based on nitride.

[0009] Preferably, in step 1), the solvothermal method comprises: mixing, stirring and ultrasonically treating a metal source, ethanol, ether and propylene glycol to obtain a milky white mixed suspension; then introducing the mixed suspension into a sealed solvent for thermal reaction at 100 to 150° C. for 12 to 24 hours, and obtaining a white solid powder of titanium oxide nanotubes by vacuum filtration, alcohol washing and drying.

[0010] Preferably, in step 1), the nitridation treatment comprises: subjecting the white solid powder of titanium oxide nanotubes to high temperature nitridation at 500-900° C. for 3-5 hours in an ammonia atmosphere to obtain hollow nitride nanotubes.

[0011] More preferably, the metal source includes titanyl sulfate, titanium trichloride, ammonium metavanadate, ammonium niobate oxalate hydrate, hexahydrate nitric acid bait, etc.; and / or the mass volume ratio of the metal source to ethanol, ether and glycerol is 1-1.34g:25-30mL:15-18mL:15-18mL.

[0012] Preferably, in step 1), the oil bath heating method comprises: mixing platinum acetylacetonate, nickel acetylacetonate, molybdenum hexacarbonyl, hexadecyltrimethylammonium bromide, oleylamine and diphenyl ether and ultrasonically treating the mixture for 30 to 60 minutes, performing an oil bath reaction, and obtaining one-dimensional Pt-based nanowires after centrifugation.

[0013] More preferably, the mass volume ratio of the platinum acetylacetonate, nickel acetylacetonate, molybdenum hexacarbonyl, hexadecyltrimethylammonium bromide, oleylamine and diphenyl ether is: 10-15 mg: 2-3 mg: 8-12 mg: 100-110 mg: 3-5 mL: 3-5 mL; and / or it also includes cobalt acetylacetonate, and the mass ratio of the cobalt acetylacetonate to platinum acetylacetonate is 8-10: 10-15.

[0014] More preferably, the reaction temperature of the oil bath reaction is 150-180° C., the heating rate is 5-10° C. / min, and the reaction time is 4-6 h.

[0015] Preferably, in step 2), the liquid phase method comprises: dissolving the nitride hollow nanotubes in ethanol or aqueous solution at a mass volume ratio of 20 mg: 25-50 mL, then stirring and slowly adding Pt-based nanowires, ultrasonicating at room temperature for 4-6 hours, collecting the solid product by centrifugation, washing with ethanol, and vacuum drying.

[0016] Preferably, in step 2), the ratio of Ar / H2 in the Ar / H2 atmosphere is 9:1, and the annealing temperature is 150-200°C (more preferably 130-180°C).

[0017] The present invention also provides a one-dimensional Pt-based nanowire catalyst supported on nitride hollow nanotubes, which is obtained by any of the above preparation methods.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1) The present invention proposes a method for preparing a metal carrier strong interaction catalyst. Nitride hollow nanotubes are used as semiconductors in the form of carriers to combine with low-loaded Pt-based nanowires to form a strong interaction between the metal and the carrier. The prepared catalyst is a one-dimensional hollow electrode material with high activity, high stability and low cost. The catalyst exhibits relatively excellent electrochemical performance in the cathode reduction reaction of oxygen. The activity of platinum per unit mass is 2 to 10 times that of commercial Pt / C catalysts. At the same time, the catalyst has extremely high stability due to the strong interaction between the metal carrier, which provides a new research solution for the industrial application of proton exchange membrane fuel cells and can be applied to high-efficiency electrocatalysis, organic catalysis, biodiagnosis and treatment, etc.

[0020] 2) This preparation method can simply realize the preparation of different nitride hollow nanotube-loaded Pt-based metal catalysts. It has simple process, convenient operation and low cost. It is a universal preparation method for nitride hollow nanotube-loaded Pt-based metal catalysts. The prepared nitride hollow nanotube-loaded Pt-based nanowire catalyst has good electrochemical activity and high stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the XRD refinement pattern of the TiN hollow nanotubes prepared in Example 1.

[0022] Figure 2 This is the TEM image of the TiN hollow nanotubes prepared in Example 1.

[0023] Figure 3 TEM image of the PtNi nanowires prepared in Example 1.

[0024] Figure 4 This is the TEM image of the PtNi / TiN catalyst prepared in Example 1.

[0025] Figure 5 This is the LSV test diagram of the PtNi / TiN catalyst prepared in Example 1.

[0026] Figure 6 This is a CV comparison chart of the PtNi / TiN catalyst prepared in Example 1 before and after the long-term stability performance test.

[0027] Figure 7 This is a LSV comparison chart of the PtNi / TiN catalyst prepared in Example 1 before and after the long-term stability performance test.

[0028] Figure 8 This is the TEM image of the Pt / TiNbN catalyst prepared in Example 2.

[0029] Fig. 9 This is a high-resolution transmission electron microscopy (HR-TEM) image of the Pt / TiNbN catalyst prepared in Example 2. DETAILED DESCRIPTION

[0030] In order to better understand the technical content of the present invention, specific embodiments are provided below and combined with the accompanying drawings to further illustrate the present invention.

[0031] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0032] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources, and the purity of the drugs is analytical grade.

[0033] Example 1: PtNi / TiN catalyst

[0034] (1) Preparation of TiN hollow nanotubes used as substrate

[0035] In a fume hood, add 25 mL of ethanol, 15 mL of ether and 15 mL of glycerol to a Montex washing bottle, then add 1 g of titanyl sulfate, stir for 2 h, rotate at 60 rpm, and ultrasonicate for 1 h. After stirring and ultrasonicating evenly, introduce into a 100 mL polytetrafluoroethylene liner sealed solvent for thermal reaction for 12 h, and the reaction temperature is 120°C; obtain TiO2 white solid powder by vacuum filtration and alcohol washing, and then put it into a blast drying oven to dry overnight to obtain TiO2 white solid powder, and the temperature of the blast drying oven is 60°C;

[0036] 1g of TiO2 white solid powder was placed in a quartz boat, which was then placed in a quartz tube furnace. High-purity nitrogen was introduced to replace the air in the furnace tube, and then ammonia water was introduced and the temperature was raised. The flow rate of ammonia water was controlled at 10mL / min, and the heating rate was 5℃ / min. The temperature was raised to 800℃ and then nitrided at this temperature for 4h. Then, high-purity nitrogen was switched and the temperature was lowered. After the temperature was lowered to room temperature, the product was taken out and refined by XRD. The obtained product was a pure faceted cubic structure of TiN( Figure 1 ).

[0037] (2) Preparation of one-dimensional PtNi nanowires

[0038] In a fume hood, 3 mL of oleylamine and 3 mL of diphenyl ether were mixed and added to a Monte Carlo washing bottle, and then 10 mg of platinum acetylacetonate, 2.1 mg of nickel acetylacetonate, 9 mg of molybdenum hexacarbonyl, and 110 mg of hexadecyltrimethylammonium bromide were added. After ultrasonic homogenization, an oil bath reaction was carried out at a temperature of 180 ° C and a reaction time of 4 h. PtNi nanowires were obtained after centrifugation.

[0039] (3) Preparation of PtNi / TiN by liquid phase method and construction of strong metal-support interaction

[0040] In a fume hood, 20 mg of TiN prepared in step (1) was dissolved in 25 mL of ethanol or aqueous solution and soaked in ultrasound for 1 h, then stirred and slowly added with the PtNi nanowires prepared in step (2), ultrasound was performed at room temperature for 4 h, and the PtNi / TiN precursor was collected by centrifugation;

[0041] Take 10 mg of PtNi / TiN precursor powder and put it into a quartz boat, put it into a quartz tube furnace, first introduce argon to replace the air in the furnace tube, and then introduce hydrogen to start heating; the ratio of argon to hydrogen is 9:1, and the heating rate is 5°C / min; heat to 130°C and then keep it at this temperature for 60 minutes, cool to room temperature and take out to obtain PtNi / TiN catalyst.

[0042] The actual composition of the catalyst can be determined by inductively coupled plasma optical emission spectroscopy (ICP-OES). The concentration is determined by ICP-OES spectroscopy, and finally the mass composition of the catalyst is converted to determine the actual loading amount of Pt.

[0043] (4) Catalyst structural morphology characterization and performance testing

[0044] (A) Structural morphology and elemental characterization:

[0045] Transmission electron microscopy (TEM) was used to observe the titanium nitride hollow nanotubes ( Figure 2 )、PtNi nanowires( Figure 3 ) and the morphology of titanium nitride loaded with PtNi nanowires ( Figure 4 ), the average diameter of the titanium nitride prepared in this embodiment is 0.8-1.5μm, the length is 12-15μm, the average diameter of the PtNi nanowire prepared is 1-2nm, the length is 10-20nm, and the PtNi nanowire is evenly distributed on the surface of the TiN carrier after loading. The results of ICP analysis show that the platinum loading of the catalyst prepared in this embodiment is 15.4wt%.

[0046] (B) Performance test:

[0047] The prepared PtNi / TiN catalyst was subjected to linear voltammetric scanning (LSV) in oxygen-saturated 0.1M HClO4 at a scan rate of 10mV / s and an electrode rotation speed of 1600r / min under a three-electrode system. The catalyst showed very excellent performance. The results are shown in Figure 5 .

[0048] Using a three-electrode system, cyclic voltammetry (CV) was performed in 0.1M HClO4 solution at a scan rate of 50mV / s. The operation was stopped after the curve stabilized and the scan curve was recorded. Subsequently, LSV scan was performed in 0.1M HClO4 saturated with oxygen and the scan curve was recorded. The changes in catalyst CV and LSV are shown in Figure 6 and Figure 7 .

[0049] The test results show that the oxygen reduction activity per unit mass of platinum of the catalyst prepared in this example is 3.4 times that of the commercial Pt / C catalyst.

[0050] Unless otherwise specified, the test methods for cathode oxygen reduction and catalyst stability of the catalyst involved in the present invention are the same as the above test methods.

[0051] Example 2: Pt nanoparticle-supported TiNbN catalyst

[0052] Except for the following steps which are different from those in Example 1, other preparation and testing methods are exactly the same as those in Example 1.

[0053] (1) Preparation of TiNbN hollow nanotubes used as substrate

[0054] In a fume hood, add 25 mL of ethanol, 15 mL of ether and 15 mL of glycerol to a Montex washing bottle, then add 1 g of titanyl sulfate and 100 mg of ammonium niobate oxalate hydrate, stir and mix thoroughly, the stirring time is 2 h, the rotation speed is 60 rpm, the ultrasonic time is 1 h, and after stirring and ultrasonication evenly, introduce into a 100 mL polytetrafluoroethylene liner sealed solvent for thermal reaction for 12 h, and the reaction temperature is 120°C; obtain TiNbO2 white solid powder by vacuum filtration and alcohol washing, and then put it into a blast drying oven to dry overnight to obtain TiNbO2 white solid powder, and the temperature of the blast drying oven is 60°C;

[0055] (2) Preparation of Pt nanoparticles

[0056] Dissolve 1 g of chloroplatinic acid in 50 mL of distilled water for later use.

[0057] (3) Preparation of Pt / TiNbN by evaporation solvent method and construction of strong metal-support interaction

[0058] Pt nanoparticles were loaded on TiMN by evaporating the solvent. Specifically, 16 mg of TiN powder was dissolved in 25 mL of ethanol or aqueous solution, and ultrasonicated for 60 min until TiNbN was evenly dispersed. Then 1 mL of chloroplatinic acid solution was added dropwise, and ultrasonicated for 60 min to ensure that Pt was evenly dispersed on TiNbN. The mixture was stirred for 4 h at a speed of 400 rpm. After stirring, the temperature was raised to 130 ° C to evaporate the solvent. After evaporation, the sample was ground and annealed at 130 ° C for 60 min at a heating rate of 5 ° C / min in an Ar / H2 (Ar: 90%, H2: 10%) atmosphere to obtain a Pt / TiNbN catalyst.

[0059] (4) Structural morphology and elemental characterization:

[0060] The morphology of the nitride loaded with Pt nanoparticles was observed by transmission electron microscopy (TEM). Figure 8 ), the average diameter of Pt nanoparticles is 5-10nm. After loading, Pt nanoparticles are evenly distributed on the surface of the TiN carrier, and after pyrolysis, due to the strong interaction between the metal carrier, the TiN carrier forms an encapsulation layer to the Pt nanoparticles ( Fig. 9 ). The results of ICP analysis showed that the platinum loading of the catalyst prepared in this example was 18.3 wt%.

[0061] The oxygen reduction activity per unit mass of platinum of the catalyst prepared in this example is 3.9 times that of the commercial Pt / C catalyst.

[0062] Example 3: PtNiCo / TiN Catalyst

[0063] Except for the following steps which are different from those in Example 1, other preparation and testing methods are exactly the same as those in Example 1.

[0064] (2) Preparation of one-dimensional PtNiCo nanowires:

[0065] In a fume hood, 3 mL of oleylamine and 3 mL of diphenyl ether were mixed and added to a Monte Carlo washing bottle. Then, 10 mg of platinum acetylacetonate, 2 mg of nickel acetylacetonate, 9 mg of cobalt acetylacetonate, 9 mg of molybdenum hexacarbonyl, and 110 mg of hexadecyltrimethylammonium bromide were added. After ultrasonic homogenization, an oil bath reaction was carried out at a temperature of 180 ° C and a reaction time of 4 h. PtNiCo nanowires were obtained after centrifugation.

[0066] The oxygen reduction performance of the catalyst prepared in this example is 4.8 times that of the commercial Pt / C catalyst.

[0067] Example 4: PtNi / TiErN catalyst

[0068] Except for the following steps which are different from those in Example 1, other preparation and testing methods are exactly the same as those in Example 1.

[0069] (1) Preparation of TiErN hollow nanotubes used as substrate

[0070] In a fume hood, add 25 mL of ethanol, 15 mL of ether and 15 mL of propylene glycol to a Montex washing bottle, then add 1 g of titanyl sulfate and 340 mg of hexahydrate nitric acid bait, stir and mix thoroughly for 2 h, the rotation speed is 60 rpm, the ultrasonic time is 1 h, and after stirring and ultrasonicating evenly, introduce into a 100 mL polytetrafluoroethylene liner sealed solvent for thermal reaction for 12 h, the reaction temperature is 120 ° C; obtain TiErO2 white solid powder by vacuum filtration and alcohol washing, and then put it into a forced air drying oven to dry overnight, the temperature of the forced air drying oven is 60 ° C.

[0071] The oxygen reduction performance of the catalyst prepared in this example is 3.5 times that of the commercial Pt / C catalyst.

[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a one-dimensional Pt-based nanowire catalyst supported by nitride hollow nanotubes, comprising: 1) preparing titanium oxide nanotubes by a solvothermal method, and obtaining nitride hollow nanotubes by nitridation treatment; One-dimensional Pt-based nanowires are obtained by an oil bath heating method, wherein the oil bath heating method comprises: mixing platinum acetylacetonate, nickel acetylacetonate, molybdenum hexacarbonyl, hexadecyltrimethylammonium bromide, oleylamine and diphenyl ether and ultrasonically treating the mixture for 30 to 60 minutes, performing an oil bath reaction, and obtaining one-dimensional Pt-based nanowires after centrifugation; 2) Loading Pt-based nanowires onto the surface of nitride hollow nanotubes by a liquid phase method, and annealing in an Ar / H2 atmosphere to obtain a one-dimensional Pt-based nanowire catalyst based on nitride, wherein the liquid phase method comprises: dissolving the nitride hollow nanotubes in ethanol or an aqueous solution at a mass volume ratio of 20 mg: 25-50 mL, then stirring and slowly adding Pt-based nanowires, ultrasonicating at room temperature for 4-6 hours, collecting the solid product by centrifugation, washing with ethanol, and vacuum drying.

2. The preparation method according to claim 1, characterized in that: In step 1), the solvothermal method includes: mixing, stirring and ultrasonically treating a metal source, ethanol, ether and propylene glycol to obtain a milky white mixed suspension; then introducing the mixed suspension into a sealed solvent for thermal reaction at 100 to 150° C. for 12 to 24 hours, and obtaining a white solid powder of titanium oxide nanotubes by vacuum filtration, alcohol washing and drying.

3. The preparation method according to claim 2, characterized in that: In step 1), the nitridation treatment comprises: subjecting the titanium oxide nanotube white solid powder to high temperature nitridation at 500-900° C. for 3-5 hours in an ammonia atmosphere to obtain nitride hollow nanotubes.

4. The preparation method according to claim 2, characterized in that: The metal source includes titanyl sulfate, titanium trichloride, ammonium metavanadate, ammonium niobate oxalate hydrate, and hexahydrate nitric acid bait; and / or the mass volume ratio of the metal source to ethanol, ether and glycerol is 1-1.34g:25-30mL:15-18mL:15-18mL.

5. The preparation method according to claim 1, characterized in that: The mass volume ratio of the platinum acetylacetonate, nickel acetylacetonate, molybdenum hexacarbonyl, hexadecyltrimethylammonium bromide, oleylamine and diphenyl ether is: 10-15 mg: 2-3 mg: 8-12 mg: 100-110 mg: 3-5 mL: 3-5 mL; and / or also includes cobalt acetylacetonate, and the mass ratio of the cobalt acetylacetonate to platinum acetylacetonate is 8-10:10-15.

6. The preparation method according to claim 1, characterized in that: The reaction temperature of the oil bath reaction is 150-180° C., the heating rate is 5-10° C. / min, and the reaction time is 4-6 hours.

7. The preparation method according to claim 1, characterized in that: In step 2), the ratio of Ar / H2 in the Ar / H2 atmosphere is 9:1, and the annealing temperature is 150-200°C.

8. A one-dimensional Pt-based nanowire catalyst supported on nitride hollow nanotubes, obtained by the preparation method according to any one of claims 1 to 7.