A method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material
By preparing C@ZrB2-SiC@CG coating on the surface of C/C composite materials, using discharge plasma sintering method and mechanical mixing technology, the problems of self-destruction and structural deterioration of the coating film are solved, and efficient anti-oxidation protection and Long-term effectiveness.
Patent Information
- Application Number
- CN202311827691.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-12-28
AI Technical Summary
The existing C/C composite antioxidant coatings are prone to oxidation at high temperatures, and there are problems of self-dissipation and structural deterioration during the coating film formation process, resulting in insufficient protection effect and aging.
The C@ZrB2-SiC inner coating was prepared by discharge plasma sintering method, and the slurry was formed by mixing borosilicate glass with nano ZrO2 powder in a silicon sol, and repeatedly brushed on the inner coating, and then under vacuum environment. Lossless film formation treatment to form a C@ZrB2-SiC@CG coating.
Lossless film formation is achieved, the coating film formation loss is avoided, the protective effect and aging are significantly improved, the formation of oxygen diffusion channels is prevented, and the service life of the coating is extended.
Smart Images

Figure CN118108530B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of C / C composite materials, and in particular to a method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material. Background Art
[0002] C / C composites have the advantages of low density, high strength, high thermal conductivity, and low expansion coefficient, and have potential uses in aerospace and other fields. However, C / C composites are very easy to oxidize at high temperatures, and oxidation protection measures must be taken when used in high-temperature aerobic environments. Coating technology is currently the most widely used and most deeply studied anti-oxidation protection technology. Ultra-high temperature ceramic borides have many advantages such as high melting point and high temperature stability, and are a very promising anti-oxidation coating system.
[0003] Among ultra-high temperature ceramic borides, ZrB2 has attracted much attention due to its high melting point, high thermal conductivity and low thermal expansion coefficient. However, one of the main oxidation products of ZrB2 coating is B2O3, and the volatilization of B2O3 usually leads to a high defect structure of the coating. SiC is often used to modify ZrB2 coating. The oxidation product of ZrB2-SiC composite ceramic coating is a borosilicate glass with greater viscosity and lower volatility. This glass can melt and flow at high temperature to form a uniform glass film, effectively inhibiting the penetration of oxygen into the coating. The formation of the glass layer usually occurs in the early stage of oxidation and takes a certain period of time to complete. This process is usually accompanied by severe oxidation of the coating, resulting in a large amount of loss of the coating itself. This self-destructive film formation method will inevitably shorten the service life of the coating. Therefore, it is of great significance to inhibit the film loss in the early stage of coating oxidation.
[0004] Chu Hongao (Chu Hongao. Preparation of ZrB2-SiC coating by spark plasma sintering and its high oxygen barrier mechanism [D]. China University of Mining and Technology, 2021.) used the spark plasma method to prepare the ZrB2-SiC oxygen barrier coating, achieving oxygen barrier protection at 1700°C. Although the coating forms a self-generated oxygen barrier glass layer on the surface after high-temperature oxidation, which can resist oxygen corrosion, the formation of the self-generated glass layer is bound to be accompanied by a large amount of film loss, and the formation of the glass layer at high temperature still requires a certain period of time, so it is impossible to form effective oxygen barrier protection at medium temperature. Relying only on the intrinsic structure of the coating for oxygen barrier protection, the oxygen barrier effect is limited. Chen Yuexing (Chen Yuexing. Research on oxygen barrier properties of binary transition metal silicide modified ZrB2 coating based on self-propagating combustion synthesis [D]. China University of Mining and Technology, 2023) pre-oxidized the TaB2-SiC coating to form a film, and prepared a Ta-B-Si-O multiphase glass layer with low oxygen permeability at low film loss under medium and high temperature oxygen annealing. However, there is still low self-damage in the film formation process, which is bound to deteriorate the coating structure. Therefore, there is an urgent need for a coating preparation technology to solve the problems of film self-damage and deterioration of coating structure in the existing technology, and to improve the coating protection effect and protection time. Summary of the invention
[0005] The present invention aims to provide a method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material, specifically a non-destructive film forming method of a C@ZrB2-SiC@CG coating, characterized in that the method is carried out according to the following steps:
[0006] (1) Preparing a C@ZrB2-SiC inner coating by spark plasma sintering according to the molar ratio;
[0007] (2) Borosilicate glass and nano ZrO2 powder were mixed into silica sol, mechanically mixed to form a slurry, and then applied on the C@ZrB2-SiC inner coating. The slurry was repeated three times and then placed in an oven for pre-drying.
[0008] (3) The pre-dried sample is placed in a tube furnace and subjected to non-destructive film forming treatment according to a preset procedure under a vacuum environment. After the treatment, it is cooled to room temperature to obtain a C@ZrB2-SiC@CG coating.
[0009] Preferably, in step (1), commercial ZrB2 powder and commercial SiC powder are used as raw materials to prepare the C@ZrB2-SiC inner coating, and the volume ratio of commercial ZrB2 powder to commercial SiC powder is 60 vol% ZrB2-40 vol% SiC.
[0010] Preferably, in step (2), the mass ratio of borosilicate glass to nano ZrO2 powder is in the range of 95:5 to 85:15.
[0011] Preferably, in step (3), the non-destructive film forming treatment time is 5 to 6 hours.
[0012] Preferably, in step (3), the non-destructive film forming treatment temperature ranges from 1200 to 1300°C.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] (1) The non-destructive film-forming method adopted in the present invention has a simple process and low equipment requirements, which ensures the preparation cycle of the coating sample and overcomes the problem of self-damage of the anti-oxidation coating film; it fundamentally avoids the coating film loss and improves the protective effect of the coating.
[0015] (2) As an effective coating preparation method, the C@ZrB2-SiC@CG coating of the present invention utilizes non-destructive film-forming technology, which avoids self-damage of film formation compared with conventional anti-oxidation coating protection technology and existing pre-oxidation film-forming technology, effectively prevents the degradation of the coating structure caused by oxidation self-damage, avoids the formation of oxygen diffusion channels in the intrinsic structure, and improves the protective effectiveness of the coating.
[0016] In summary, the present invention overcomes the problems of conventional anti-oxidation coating protection technology and existing pre-oxidation film-forming technology, such as film self-damage and deteriorated coating structure, and has the characteristics of simple process, strong applicability, non-destructive film formation, and significant anti-oxidation protection effect; it fundamentally avoids the coating film loss, improves the protection effect of the coating, effectively prevents the degradation of the coating structure caused by oxidation self-damage, avoids the formation of oxygen diffusion channels in the intrinsic structure, and improves the protection time of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the process of the present invention.
[0018] Figure 2 This is a scanning electron microscope morphology image of the C@ZrB2-SiC@CG coating obtained in Example 1 of the present invention.
[0019] Figure 3 This is a scanning electron microscope morphology image of the C@ZrB2-SiC@CG coating obtained in Example 2 of the present invention.
[0020] Figure 4 This is a scanning electron microscope morphology image of the C@ZrB2-SiC@CG coating obtained in Example 3 of the present invention.
[0021] Figure 5 This is a scanning electron microscope morphology image of the ZrB2-SiC coating obtained in Comparative Example 1 of the present invention.
[0022] Figure 6This is a scanning electron microscope morphology image of the pre-oxidized film-forming ZrB2-SiC coating obtained in Comparative Example 2 of the present invention.
[0023] Figure 7 The oxidation weight gain results of the C@ZrB2-SiC@CG coatings obtained in Examples 1 to 3 of the present invention and the self-destructive film-forming coatings of Comparative Examples 1 to 2 are shown.
[0024] Figure 8 These are the protection efficiency results of the C@ZrB2-SiC@CG coatings obtained in Examples 1 to 3 of the present invention and the self-destructive film-forming coatings of Comparative Examples 1 to 2. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0026] Embodiment 1:
[0027] A method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material is carried out according to the following steps:
[0028] (1) According to the molar ratio, the C@ZrB2-SiC inner coating was prepared by spark plasma sintering, specifically: commercial ZrB2 powder and commercial SiC powder were used as raw materials, according to the volume ratio of 60 vol% ZrB2-40 vol% SiC, and the C@ZrB2-SiC inner coating was sintered at 1500°C by spark plasma sintering;
[0029] (2) borosilicate glass and nano ZrO2 powder were mixed into silica sol in a ratio of 95:5, mechanically mixed to form a slurry, and then applied on the C@ZrB2-SiC inner coating. The slurry was repeated three times and then placed in an oven for pre-drying.
[0030] (3) The pre-dried sample was placed in a tube furnace and subjected to non-destructive film forming treatment under vacuum according to a preset procedure (treatment time 5 h, treatment temperature 1200 °C). After the treatment, it was cooled to room temperature to obtain the C@ZrB2-SiC@CG coating.
[0031] The cross-sectional microstructure of the obtained C@ZrB2-SiC@CG coating is shown in Figure 2 As shown, the oxidation weight gain results and cumulative protection efficiency are as follows Figure 7 and Figure 8 The results of oxidation weight gain and oxidation protection efficiency at 1700°C are shown in Table 1.
[0032] Embodiment 2:
[0033] A method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material is carried out according to the following steps:
[0034] (1) According to the molar ratio, the C@ZrB2-SiC inner coating was prepared by spark plasma sintering; the specific method was the same as that in Example 1;
[0035] (2) borosilicate glass and nano ZrO2 powder were mixed into silica sol in a ratio of 90:10, mechanically mixed to form a slurry, and applied to the C@ZrB2-SiC inner coating. The slurry was repeated three times and then placed in an oven for pre-drying.
[0036] (3) The pre-dried sample was placed in a tube furnace and subjected to non-destructive film forming treatment under vacuum according to a preset procedure (treatment time 5.5 h, treatment temperature 1250 °C). After the treatment, it was cooled to room temperature to obtain the C@ZrB2-SiC@CG coating.
[0037] The cross-sectional microstructure of the obtained C@ZrB2-SiC@CG coating is shown in Figure 3 As shown, the oxidation weight gain results and cumulative protection efficiency are as follows Figure 7 and Figure 8 The results of oxidation weight gain and oxidation protection efficiency at 1700°C are shown in Table 1.
[0038] Embodiment 3:
[0039] A method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material is carried out according to the following steps:
[0040] (1) According to the molar ratio, the C@ZrB2-SiC inner coating was prepared by spark plasma sintering; the specific method was the same as that in Example 1;
[0041] (2) borosilicate glass and nano ZrO2 powder were mixed into silica sol in a ratio of 85:15, mechanically mixed to form a slurry, and applied to the C@ZrB2-SiC inner coating. The slurry was repeated three times and then placed in an oven for pre-drying.
[0042] (3) The pre-dried sample was placed in a tube furnace and subjected to non-destructive film forming treatment according to a preset procedure under a vacuum environment (treatment time: 6 h, treatment temperature: 1300 °C). After the treatment, it was cooled to room temperature to obtain a C@ZrB2-SiC@CG coating.
[0043] The cross-sectional microstructure of the obtained C@ZrB2-SiC@CG coating is shown in Figure 4 As shown, the oxidation weight gain results and cumulative protection efficiency are as follows Figure 7 and Figure 8The results of oxidation weight gain and oxidation protection efficiency at 1700°C are shown in Table 1.
[0044] Comparative Example 1:
[0045] The C@ZrB2-SiC inner coating was prepared by spark plasma sintering according to the molar ratio, specifically: commercial ZrB2 powder and commercial SiC powder were used as raw materials, and the ratio of 60 vol% ZrB2-40 vol% SiC was sintered at 1500°C by spark plasma sintering to obtain the C@ZrB2-SiC inner coating;
[0046] Comparative Example 1 Cross-sectional microstructure Figure 5 As shown in the figure, the 1700℃ antioxidant performance and cumulative protection efficiency are as follows: Figure 7 and Figure 8 The results of oxidation weight gain and oxidation protection efficiency at 1700°C are shown in Table 1. It can be found that:
[0047] Compared with Example 1, Comparative Example 1 did not perform any film-forming treatment on the ZrB2-SiC coating. Since it relied solely on the coating structure to block oxygen and lacked the protection of the composite glass layer, Comparative Example 1 had an obvious rapid weight gain stage at 600°C-800°C, and the coating was severely oxidized. Compared with Examples 1 to 3 of the present invention, Comparative Example 1 was most severely oxidized at 1700°C, had the largest oxidation weight gain, and had the worst protection effect.
[0048] Comparative Example 2:
[0049] (1) preparing a C@ZrB2-SiC inner coating by spark plasma sintering according to the molar ratio;
[0050] (2) The C@ZrB2-SiC inner coating was pre-oxidized and film-formed in a muffle furnace (film-forming temperature 1300°C, film-forming time 6h) to obtain a C@ZrB2-SiC@CG coating.
[0051] Comparative Example 2 Cross-sectional microstructure Figure 6 As shown in the figure, the 1700℃ antioxidant performance and cumulative protection efficiency are as follows: Figure 7 and Figure 8 The results of oxidation weight gain and oxidation protection efficiency at 1700°C are shown in Table 1. It can be found that:
[0052] Compared with Example 3, Comparative Example 2 uses a traditional pre-oxidation film-forming process to prepare a glass layer. Since the traditional pre-oxidation film-forming process has intrinsic film loss of the coating, that is, the protective effect itself is shortened. In addition, the Si loss of the coating obtained in Comparative Example 2 is significantly more serious, that is, there are internal defects and oxygen diffusion channels when the coating is lost during film formation. The weight gain per unit area after the same oxidation conditions (oxidation temperature, oxidation time) is greater than that of the embodiments, indicating that the degree of oxidation and loss are more serious, that is, the embodiments of the present invention have more excellent protective effects and effectiveness.
[0053] Table 1 Results of oxidation weight gain and oxidation protection efficiency at 1700℃
[0054]
[0055] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.
Claims
1. A method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material, specifically a non-destructive film forming method of a C@ZrB2-SiC@CG coating, characterized in that: The following steps were followed: (1) a C@ZrB2-SiC inner coating was prepared by spark plasma sintering according to a molar ratio; (2) Borosilicate glass and nano ZrO2 powder were mixed into silica sol, mechanically mixed to form a slurry, and then applied on the C@ZrB2-SiC inner coating. The slurry was repeated three times and then placed in an oven for pre-drying. (3) placing the pre-dried sample into a tube furnace and performing non-destructive film forming treatment under vacuum according to a preset procedure, and cooling to room temperature after the treatment to obtain a C@ZrB2-SiC@CG coating; In the step (2), the mass ratio of borosilicate glass to nano ZrO2 powder is in the range of 95:5 to 85:15; In the step (3), the non-destructive film forming treatment time is 5 to 6 hours; In the step (3), the non-destructive film forming treatment temperature ranges from 1200 to 1300°C.
2. The method for preparing a gradient anti-oxidation coating on the surface of a C / C composite material according to claim 1, characterized in that: In the step (1), commercial ZrB2 powder and commercial SiC powder are used as raw materials to prepare the C@ZrB2-SiC inner coating, and the volume ratio of the commercial ZrB2 powder and the commercial SiC powder is 60 vol% ZrB2-40 vol% SiC.