A high temperature resistant bio-based furan resin binder and preparation method thereof

By using a composite material of yttrium aluminum garnet micropowder and gradient material coating mullite whiskers in furan resin, the problem of insufficient high temperature resistance of furan resin sand is solved, and the high temperature resistance and thermal stability of the resin are improved to ensure Castings maintain strength and dimensional accuracy at high temperatures, reduce defects, and improve casting quality and production efficiency.

CN118122944BActive Publication Date: 2024-10-11SUZHOU XINGYE MATERIALS TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410318206.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2024-10-11
Estimated Expiration
2044-03-20

AI Technical Summary

Technical Problem

Furan resin sand has insufficient high-temperature resistance, which causes castings to be easily deformed at high temperatures and has poor pyrolysis performance, affecting the quality and production efficiency of castings.

Method used

Yttrium aluminum garnet micropowder and gradient material are used to coat mullite whiskers to form a composite material, which is combined in furan resin. Through the thermal stress relaxation of the gradient material and the high temperature creep resistance of yttrium aluminum garnet, the resin's resistance is improved. High temperature resistance and thermal stability.

Benefits of technology

It effectively prevents cracks and shrinkage of resin, improves its strength and high temperature resistance, delays pyrolysis, ensures that castings maintain strength and dimensional accuracy at high temperatures, reduces defects, and improves the quality and production efficiency of castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004749659360000111
    Figure BDA0004749659360000111
  • Figure BDA0004749659360000121
    Figure BDA0004749659360000121
  • Figure BDA0004749659360000122
    Figure BDA0004749659360000122
Patent Text Reader

Abstract

The present invention provides a high temperature resistant bio-based furan resin binder and a preparation method thereof. The method comprises the following steps: adding furfuryl alcohol and furfural into a reactor for stirring, adding an organic acid for continuous stirring; heating for reaction; cooling, adding sodium hydroxide, adjusting the pH value, and vacuum dehydration; adding 5-HMF and a silane coupling agent for stirring evenly; adding gradient material-coated mullite whiskers and yttrium aluminum garnet micropowder for stirring evenly. The present invention adopts yttrium aluminum garnet micropowder to compound with gradient material-coated mullite whiskers. The gradient material-coated mullite whiskers can play a role in pinning resin cracks and inhibiting shrinkage during curing, effectively preventing the occurrence of cracks and shrinkage, and is conducive to improving its high temperature resistance; the pyrolysis temperature of yttrium aluminum garnet micropowder and gradient material-coated mullite whiskers is not completely synchronized. As the temperature rises, the heat transfer and digestion of the two can help to delay the pyrolysis of furan resin, thereby further improving thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional resins, and in particular to a high-temperature resistant bio-based furan resin binder and a preparation method thereof. Background Art

[0002] In the late 1960s, various resin sands represented by furan resin sand emerged and attracted widespread attention from foundries around the world. Various resin sands were introduced and promoted, which led to major changes in the methods of modeling and core making. A large number of castings originally produced with clay sand and water glass sand, especially medium and large castings produced in small batches, have been replaced by resin sands, which has brought obvious technical, economic and social benefits to many enterprises. The use of furan resin sand to make sand molds (cores) and cast castings has high dimensional accuracy, good surface finish, low scrap rate, and can realize the mechanized assembly line production of small and medium batches of complex castings. Due to its excellent performance, furan resin sand has been rapidly applied in casting production. Although various molding processes coexist due to different scopes of use, resin sand still has an absolute advantage, among which self-hardening resin sand has developed the fastest, but it also has certain defects. The preparation process of furan resin sand: curing agent + sand mixed + resin mixed to make a mixture and then molded, after molding (sand mold and sand core) combined, painted, and high-temperature molten iron poured into castings. If the high-temperature resistance of the sand mold is poor, the casting is easy to deform during pouring. Therefore, it is also necessary to improve the high-temperature resistance of the furan resin binder. Summary of the invention

[0003] Technical problem to be solved: In view of the above technical problems, the purpose of the present invention is to provide a high-temperature resistant bio-based furan resin binder and a preparation method thereof, wherein yttrium aluminum garnet powder is used to compound with gradient material-coated mullite whiskers, the gradient material-coated mullite whiskers, the mullite whiskers are fibrous, coated and combined with the furan resin, and can play a role in pinning resin cracks and inhibiting shrinkage during curing, effectively preventing the occurrence of cracks and shrinkage, helping to improve the strength of the furan resin, and also helping to improve its high temperature resistance; yttrium aluminum garnet itself has extremely high high-temperature creep resistance, so it can improve the high temperature resistance of the furan resin, and at the same time, the pyrolysis temperature of the yttrium aluminum garnet powder and the gradient material-coated mullite whiskers are not completely synchronized, with the increase of temperature, the heat transfer and digestion between the two can help to delay the pyrolysis of the furan resin, thereby further improving the thermal stability, and the fibrous gradient material-coated mullite whiskers and the granular yttrium aluminum garnet powder also play a complementary role in mechanical properties.

[0004] Technical solution: A high-temperature resistant bio-based furan resin binder, comprising the following components, by weight: 50-80 parts of furfuryl alcohol, 40-50 parts of furfural, 10-20 parts of 5-hydroxymethylfurfural (5-HMF), 0.3-0.6 parts of silane coupling agent, 8-12 parts of gradient material coated mullite whiskers, 3-5 parts of yttrium aluminum garnet powder, 0.2-0.4 parts of organic acid, and 0.2-0.4 parts of sodium hydroxide.

[0005] Furthermore, the preparation method of the gradient material coated mullite whisker is:

[0006] S1: stirring and mixing the mullite whisker and the composite gradient material to obtain a mixture;

[0007] S2: Place the mixture in a wet mixer, add grinding media, and grind for 30-45 minutes to obtain.

[0008] Furthermore, the diameter of the mullite whisker is 1-2 μm, and the aspect ratio is 20-30.

[0009] Furthermore, the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of (2-3):2:1.

[0010] Furthermore, the mass ratio of the mullite whisker to the composite gradient material is (2-3):(3-2).

[0011] Furthermore, the grinding media are ceramic microbeads with diameters of 20 μm, 35 μm, 50 μm and 80 μm respectively in a volume ratio of 1:2:1:1, and the mass ratio of the grinding media to the mixed material is (4-5):1.

[0012] Furthermore, the particle size of the yttrium aluminum garnet powder is 0.5-1 μm.

[0013] Furthermore, the organic acid includes phosphoric acid, oxalic acid and citric acid.

[0014] The preparation method of the above-mentioned high temperature resistant bio-based furan resin binder comprises the following steps:

[0015] (1) adding furfuryl alcohol and furfural into a reaction kettle and stirring, then adding an organic acid and continuing stirring for 15-20 minutes;

[0016] (2) heating to 100-120°C and reacting for 3-4 hours;

[0017] (3) cooling to below 70° C., adding sodium hydroxide, adjusting the pH value to 7, and vacuum dehydrating;

[0018] (4) adding 5-hydroxymethylfurfural and silane coupling agent and stirring evenly;

[0019] (5) adding gradient material coated mullite whiskers and yttrium aluminum garnet powder and stirring evenly;

[0020] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0021] Furthermore, in the heating process of step (2), the viscosity is measured once every hour for the first 2 hours, and once every 0.5 hours after 2 hours. When the viscosity at 70°C reaches 15 seconds, the viscosity is measured once every 10 minutes. When the viscosity at 70°C reaches 16-17 seconds, the cooling of step (3) is immediately performed.

[0022] Furthermore, in the step (3), the vacuum degree is greater than 825 kPa and the dehydration temperature is less than or equal to 68°C.

[0023] Beneficial effects:

[0024] 1. The present invention adopts gradient material to coat mullite whiskers. The mullite whiskers are fibrous and are coated and combined with bio-based furan resin. During curing, they can play a role in pinning the furan resin cracks and inhibiting shrinkage, effectively preventing the occurrence of cracks and shrinkage, helping to improve the strength of the furan resin, and also helping to improve its high temperature resistance.

[0025] 2. The present invention uses gradient materials to coat mullite whiskers. Since the thermal stress curves and thermal expansion coefficients of MoSi2 powder, Cr2O3 powder and Cr powder are different, thermal stress relaxation can be achieved when encountering high temperatures. When the resin sand is subjected to high temperatures, the thermal expansion of the resin sand can be relaxed, effectively preventing the casting from producing thermal cracking defects, and ensuring that the molding sand maintains a certain strength at high temperatures without causing the sand mold to be damaged prematurely and causing defects such as sand blasting, ultimately obtaining high-quality castings with fewer defects; and since MoSi2 has the common characteristics of metallic bonds and covalent bonds, it is an ultra-high temperature resistant material and can be better combined with furan resin, thereby improving the high temperature resistance of the furan resin.

[0026] 3. In the present invention, yttrium aluminum garnet micropowder is used to compound with gradient material coated mullite whiskers. Since yttrium aluminum garnet itself has extremely high high-temperature creep resistance, it can improve the high temperature resistance of furan resin. At the same time, the pyrolysis temperature of yttrium aluminum garnet micropowder and gradient material coated mullite whiskers are not completely synchronized. As the temperature increases, the heat transfer and digestion between the two can help delay the pyrolysis of furan resin, thereby further improving thermal stability. In addition, the fibrous gradient material coated mullite whiskers and the granular yttrium aluminum garnet micropowder also play a complementary role in mechanical properties.

[0027] 4. In the present invention, at high temperature, the surface of the furan resin will combine with the yttrium aluminum garnet powder and the gradient material-coated mullite whiskers to form a dense continuous layer covering the resin surface, thereby further improving the high temperature resistance. DETAILED DESCRIPTION

[0028] The present invention proposes a high temperature resistant bio-based furan resin binder and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention will be further described in detail with reference to the following examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not intended to limit the present invention.

[0029] Experimental Materials

[0030] Mullite whiskers (diameter: 1-2μm, aspect ratio: 20-30); yttrium aluminum garnet powder (particle size: 0.5-1μm); MoSi2 powder (particle size: 100-300nm); Cr2O3 powder (particle size: ≤3μm); Cr powder (particle size: ≤3μm); ceramic microbeads (diameters are 20μm, 35μm, 50μm and 80μm respectively); furfural: content >96%; furfuryl alcohol: content >98%; oxalic acid: white crystals, purity >99.0%; silane coupling agent kh560 >97.0%.

[0031] Example 1

[0032] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0033] (1) adding 50 parts of furfuryl alcohol and 40 parts of furfural into a reaction kettle and stirring, then adding 0.2 parts of oxalic acid and continuing stirring for 15 minutes; (2) heating to 110°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0034] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0035] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0036] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0037] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0038] The preparation method of gradient material coated mullite whiskers is as follows:

[0039] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0040] S2: Place the mixture in a wet mixer, add grinding media, the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1, and the mass ratio of the grinding media to the mixture is 4:1, and grind for 30 minutes.

[0041] Example 2

[0042] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0043] (1) adding 50 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.3 parts of oxalic acid and continuing stirring for 15 minutes; (2) heating to 110°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0044] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0045] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0046] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0047] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0048] The preparation method of gradient material coated mullite whiskers is as follows:

[0049] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0050] S2: Place the mixture in a wet mixer, add grinding media, the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1, and the mass ratio of the grinding media to the mixture is 4:1, and grind for 30 minutes.

[0051] Example 3

[0052] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0053] (1) adding 80 parts of furfuryl alcohol and 40 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 18 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0054] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0055] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0056] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0057] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0058] The preparation method of gradient material coated mullite whiskers is as follows:

[0059] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0060] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 4:1. Grind for 40 minutes to obtain the product.

[0061] Example 4

[0062] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0063] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0064] (3) Cooling to below 70°C, adding 0.4 parts of sodium hydroxide, adjusting the pH value to 7, and vacuum dehydration, the vacuum degree is 830 kPa, and the dehydration temperature is 67°C;

[0065] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0066] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0067] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0068] The preparation method of gradient material coated mullite whiskers is as follows:

[0069] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0070] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0071] Example 5

[0072] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0073] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0074] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0075] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0076] (5) adding 8 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0077] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0078] The preparation method of gradient material coated mullite whiskers is as follows:

[0079] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0080] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0081] Example 6

[0082] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0083] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0084] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0085] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0086] (5) Add 10 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stir evenly;

[0087] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0088] The preparation method of gradient material coated mullite whiskers is as follows:

[0089] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0090] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0091] Example 7

[0092] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0093] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0094] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0095] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0096] (5) adding 12 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0097] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0098] The preparation method of gradient material coated mullite whiskers is as follows:

[0099] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0100] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0101] Example 8

[0102] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0103] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0104] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0105] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0106] (5) adding 11 parts of gradient material coated mullite whiskers and 3 parts of yttrium aluminum garnet powder and stirring evenly;

[0107] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0108] The preparation method of gradient material coated mullite whiskers is as follows:

[0109] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0110] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0111] Example 9

[0112] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0113] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0114] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0115] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0116] (5) adding 11 parts of gradient material coated mullite whiskers and 5 parts of yttrium aluminum garnet powder and stirring evenly;

[0117] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0118] The preparation method of gradient material coated mullite whiskers is as follows:

[0119] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0120] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0121] Example 10

[0122] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0123] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0124] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0125] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0126] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0127] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0128] The preparation method of gradient material coated mullite whiskers is as follows:

[0129] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 2:3 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0130] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0131] Embodiment 11

[0132] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0133] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0134] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 678°C;

[0135] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0136] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0137] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0138] The preparation method of gradient material coated mullite whiskers is as follows:

[0139] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 2:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0140] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0141] Example 12

[0142] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0143] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0144] (3) Cooling to below 70°C, adding sodium hydroxide, adjusting the pH value to 7, vacuum dehydration, vacuum degree 830 kPa, dehydration temperature 67°C;

[0145] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0146] (5) adding 11 parts of gradient material coated mullite whiskers and 4 parts of yttrium aluminum garnet powder and stirring evenly;

[0147] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0148] The preparation method of gradient material coated mullite whiskers is as follows:

[0149] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 2:2:1;

[0150] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0151] Comparative Example 1

[0152] The difference between this embodiment and embodiment 4 is that the gradient material-coated mullite whiskers are replaced with an equal amount of yttrium aluminum garnet powder, specifically:

[0153] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0154] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0155] (3) Cooling to below 70°C, adding 0.4 parts of sodium hydroxide, adjusting the pH value to 7, and vacuum dehydration, the vacuum degree is 830 kPa, and the dehydration temperature is 67°C;

[0156] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0157] (5) Add 15 parts of yttrium aluminum garnet powder and stir evenly;

[0158] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0159] Comparative Example 2

[0160] The difference between this embodiment and embodiment 4 is that the yttrium aluminum garnet powder is replaced with an equal amount of gradient material coated mullite whiskers, specifically:

[0161] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0162] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0163] (3) Cooling to below 70°C, adding 0.4 parts of sodium hydroxide, adjusting the pH value to 7, and vacuum dehydration, the vacuum degree is 830 kPa, and the dehydration temperature is 67°C;

[0164] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0165] (5) Add 15 parts of gradient material to coat mullite whiskers and stir evenly;

[0166] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0167] The preparation method of gradient material coated mullite whiskers is as follows:

[0168] S1: mixing mullite whiskers and a composite gradient material in a mass ratio of 3:2 to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of 3:2:1;

[0169] S2: Place the mixture in a wet mixer and add grinding media, wherein the grinding media is ceramic micro beads with a volume ratio of 1:2:1:1 and a mass ratio of the grinding media to the mixture of 5:1, and grind for 45 minutes to obtain.

[0170] Comparative Example 3

[0171] The difference between this embodiment and embodiment 4 is that the mullite whiskers are directly used instead of being coated with gradient materials, specifically:

[0172] A method for preparing a high temperature resistant bio-based furan resin comprises the following steps:

[0173] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0174] (3) Cooling to below 70°C, adding 0.4 parts of sodium hydroxide, adjusting the pH value to 7, and vacuum dehydration, the vacuum degree is 830 kPa, and the dehydration temperature is 67°C;

[0175] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0176] (5) Add 11 parts of mullite whiskers and 4 parts of yttrium aluminum garnet powder and stir evenly;

[0177] (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0178] Comparative Example 4

[0179] The difference between this embodiment and embodiment 4 is that no gradient material is added to coat the mullite whiskers and yttrium aluminum garnet powder, specifically:

[0180] A method for preparing a bio-based furan resin comprises the following steps:

[0181] (1) adding 80 parts of furfuryl alcohol and 50 parts of furfural into a reaction kettle and stirring, then adding 0.4 parts of oxalic acid and continuing stirring for 20 minutes; (2) heating to 120°C for reaction; during the first 2 hours of heating, measuring the viscosity once every hour, after 2 hours, measuring the viscosity once every 0.5 hours, when the viscosity at 70°C reaches 15 seconds, measuring the viscosity once every 10 minutes, and when the viscosity at 70°C reaches 16-17 seconds, immediately executing step (3);

[0182] (3) Cooling to below 70°C, adding 0.4 parts of sodium hydroxide, adjusting the pH value to 7, and vacuum dehydration, the vacuum degree is 830 kPa, and the dehydration temperature is 67°C;

[0183] (4) Add 15 parts of 5-hydroxymethylfurfural and 0.5 parts of silane coupling agent KH560 and stir evenly;

[0184] (5) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

[0185] According to the standard JB / T7526-2008, the performance indicators of high temperature resistant bio-based furan resin were measured, and the results are shown in the following table:

[0186] Table 1 Conventional performance indicators of high temperature resistant bio-based furan resin

[0187]

[0188]

[0189] Take the high temperature resistant bio-based furan resin of some examples, add the curing agent, stir well, put it into a vacuum drying oven, vacuum cure it at 80°C, and use a thermogravimetric analyzer to measure its thermal stability. The test temperature is increased from 30°C to 1100°C, the heating rate is 10°C / min, and the nitrogen atmosphere is 20mL / min (the temperature when the weight loss is 10% (T 10% ), maximum thermal degradation temperature (T max ) and mass retention rate at 1100℃).

[0190] Table 2 High temperature resistance of bio-based furan resin after curing

[0191] <![CDATA[T 10% (℃)]]> <![CDATA[T max (℃)]]> Carbon residue rate (%) Example 4 307.4 515.8 60.3 Example 5 278.9 496.3 56.2 Example 6 294.3 510.4 59.1 Example 7 308.1 516.0 60.4 Example 8 300.6 510.9 58.9 Example 9 308.2 516.7 60.2 Example 10 281.6 507.1 57.3 Embodiment 11 293.4 511.6 59.2 Example 12 303.8 512.0 59.4 Comparative Example 1 293.6 510.3 59.0 Comparative Example 2 242.4 452.3 54.2 Comparative Example 3 256.1 473.5 55.5 Comparative Example 4 202.3 431.3 52.9

[0192] The Shore hardness, tensile properties (according to GB / T2567-2008 standard, the test rate is set to 2 mm / min. The tensile strength and elongation at break of the composite material are obtained by tensile testing) and compression properties (according to GB / T2569-2000 standard, the specimen shape is cylindrical, and the test rate is set to 2 mm / min) of the cured bio-based furan resin are measured.

[0193] Table 3 Mechanical properties of bio-based furan resin after curing

[0194]

[0195]

[0196] It can be seen from Table 1 that the viscosity and bonding strength of the high temperature resistant bio-based furan resin prepared by the present invention have no significant effect after adding the gradient material coated mullite whiskers and yttrium aluminum garnet powder. However, it can be seen from Tables 2 and 3 that the temperature resistance of each embodiment is significantly improved. 10% The highest temperature can reach 308.1℃, which is higher than the initial T 10% The 202.3 of the composite material has been greatly improved. At the same time, it can be seen from the experimental data that the gradient material coated with mullite whiskers and yttrium aluminum garnet powder also has the effect of enhancing the mechanical properties.

[0197] Preparation of high temperature resistant resin sand: Mix regenerated sand: high temperature resistant bio-based furan resin: curing agent in a ratio of 100:1:0.5, fill the mixed resin sand into the sample tube, pound it 3 times with a hammer-type sample making machine to make a Ф30mm×50mm cylindrical compressive strength specimen, and conduct the test after hardening.

[0198] High temperature compressive strength: Raise the furnace temperature of the high temperature strength tester to the specified temperature (respectively 1200℃ for 2min, 1000℃ for 2min, 800℃ for 3min and 600℃ for 5min), put the sample to be tested into the heating furnace, and keep it at this temperature until the center of the sample reaches the furnace temperature. The holding time varies with the specified temperature, and the holding time is longer at low temperatures. Then, press the load button to start loading until the sample is destroyed. The recording part of the tester records the maximum load value, and the high temperature compressive strength of the resin sand is obtained.

[0199] Table 4 High temperature resistance of high temperature resistant resin sand

[0200]

[0201]

[0202] It can be seen from Table 4 that after being kept at 1200℃ for 2min, the high temperature resistant resin sand still has a compressive strength of 0.47MPa. It can be seen that the high temperature resistant resin sand has good high temperature performance to ensure that the sand mold is not damaged and obtain castings with high dimensional accuracy and good surface quality.

Claims

1. A high temperature resistant bio-based furan resin binder, characterized in that: The composition comprises the following components in parts by weight: 50-80 parts of furfuryl alcohol, 40-50 parts of furfural, 10-20 parts of 5-hydroxymethylfurfural, 0.3-0.6 parts of silane coupling agent, 8-12 parts of gradient material coated mullite whiskers, 3-5 parts of yttrium aluminum garnet powder, 0.2-0.4 parts of organic acid, and 0.2-0.4 parts of sodium hydroxide; The preparation method of the gradient material coated mullite whisker is: S1: stirring and mixing the mullite whisker and the composite gradient material to obtain a mixture; the composite gradient material is MoSi2 powder, Cr2O3 powder and Cr powder in a mass ratio of (2-3):2:1; S2: Place the mixture in a wet mixer, add grinding media, and grind for 30-45 minutes to obtain.

2. A high temperature resistant bio-based furan resin binder according to claim 1, characterized in that: The diameter of the mullite whisker is 1-2 μm, and the aspect ratio is 20-30.

3. A high temperature resistant bio-based furan resin binder according to claim 1, characterized in that: The mass ratio of the mullite whisker to the composite gradient material is (2-3): (3-2).

4. The high temperature resistant bio-based furan resin binder according to claim 1, characterized in that: The grinding media are ceramic micro beads with diameters of 20 μm, 35 μm, 50 μm and 80 μm respectively in a volume ratio of 1:2:1:1, and the mass ratio of the grinding media to the mixed material is (4-5):

1.

5. The high temperature resistant bio-based furan resin binder according to claim 1, characterized in that: The particle size of the yttrium aluminum garnet powder is 0.5-1 μm.

6. The method for preparing a high temperature resistant bio-based furan resin binder according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Add furfuryl alcohol and furfural into a reactor and stir, then add organic acid and continue stirring for 15-20 minutes; (2) Heat to 100-120°C and react for 3-4 hours; (3) Cool down to below 70°C, add sodium hydroxide, adjust the pH value to 7, and perform vacuum dehydration; (4) Add 5-hydroxymethylfurfural and silane coupling agent and stir evenly; (5) Add gradient material coated mullite whiskers and yttrium aluminum garnet powder and stir evenly; (6) Cool down to 30°C, stop stirring for 20 min, and discharge the material.

7. The method for preparing a high temperature resistant bio-based furan resin binder according to claim 6, characterized in that: In the heating process of step (2), the viscosity is measured once every hour for the first 2 hours, and once every 0.5 hours after 2 hours. When the viscosity at 70°C reaches 15 s, the viscosity is measured once every 10 minutes. When the viscosity at 70°C reaches 16-17 s, the cooling of step (3) is immediately performed.

8. The method for preparing a high temperature resistant bio-based furan resin binder according to claim 6, characterized in that: In the step (3), the vacuum degree is greater than 825 kPa and the dehydration temperature is less than or equal to 68°C.

Citation Information

Cited By

  • Graphene oxide composite modified furan resin and preparation process thereof

    CN122541660A