A graphene-doped carbon-supported platinum-carbon catalyst material, a preparation method thereof, and application in hydrogen fuel cells

Graphene-doped carbon aerogels were prepared by the sol-gel method as a platinum-carbon catalyst carrier, which solved the problems of deactivation and electrochemical corrosion of traditional catalysts in hydrogen fuel cells and achieved high efficiency, stability and improved performance of the catalyst.

CN118136869BActive Publication Date: 2024-10-15ANHUI RUIHE POWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410360905.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-15
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

The Pt/C catalyst commonly used in traditional hydrogen fuel cells is easily deactivated in harsh environments. The surface structure and components of the carbon carrier affect the stability of the catalyst, and commercial carbon black is susceptible to electrochemical corrosion, leading to catalyst deactivation and affecting electrochemical performance. Heap performance.

Method used

Graphene-doped carbon aerogels are prepared using the sol-gel method as a platinum carbon catalyst carrier. The electrochemical corrosion resistance and catalytic activity of the catalyst are improved through graphene modification, forming a petal-shaped catalyst with a multi-layer structure to enhance the stability of the catalyst. properties and active site exposure.

Benefits of technology

It significantly improves the durability and catalytic performance of the catalyst, enhances the long-term cycle stability for oxygen reduction reactions, and reduces electrochemical corrosion, making it suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118136869B_ABST
    Figure CN118136869B_ABST
Patent Text Reader

Abstract

The present invention provides a graphene-doped carbon-supported platinum-carbon catalyst material, a preparation method thereof, and an application in a hydrogen fuel cell. Carbon aerogel CA is prepared by a sol-gel method, and has better electrochemical corrosion resistance. Platinum nanoparticles are loaded on CA, and the prepared Pt / CA has higher catalytic activity and better ORR long-term cycle stability. In addition, the present invention modifies the carbon aerogel material by graphene. After the graphene is doped with the carbon aerogel, the single-level structure is transitioned to a hierarchical structure, and the presence of graphene inhibits its shrinkage, resulting in a part of the carbon aerogel nanoparticles being attached to the graphene surface during the carbonization process, and the other part being distributed in the gaps of the graphene sheet in the form of microparticles. The close bonding and synergistic coupling effect between the graphene and the nanoparticles loaded thereon make the graphene-based composite material have higher oxygen reduction catalytic activity and catalyst carrier stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy battery materials, and specifically relates to a graphene-doped carbon-supported platinum-carbon catalyst material, a preparation method thereof, and an application in a hydrogen fuel cell. Background Art

[0002] In recent years, the massive consumption of traditional energy has led to an increasingly severe energy crisis, and the resulting environmental pollution problems have also followed one after another. People are in urgent need of a new type of clean energy to replace traditional energy. As we all know, hydrogen is a clean energy with many advantages, such as high calorific value, no pollution in products and abundant reserves.

[0003] A hydrogen fuel cell is a power generation device that can directly convert the chemical energy of hydrogen into electrical energy. Its large-scale commercial use can alleviate the environmental pollution problems caused by the use of traditional energy and realize the vision of clean energy transformation in the future.

[0004] The catalyst layer in a hydrogen fuel cell is the place where hydrogen and oxygen undergo electrochemical reactions to generate current, and is the core of the hydrogen fuel cell. At present, the most commonly used cathode and anode catalysts in hydrogen fuel cells are Pt / C catalysts, but the harsh working environment of hydrogen fuel cells can easily lead to catalyst degradation and loss of activity. Among the many factors that lead to catalyst electrocatalytic deactivation, the surface structure and composition of the carbon carrier are one of the most important influencing factors. Commercial carbon black has been widely used as a carrier material for Pt / C catalysts due to its low cost, high availability and high mesoporous distribution. However, this carbon material is prone to electrochemical corrosion at defects and edges, and its weak interaction with platinum nanoparticles will cause the migration and aggregation of platinum during the catalytic process. All of the above will lead to catalyst deactivation, thereby affecting the comprehensive performance of the membrane electrode and the final stack product.

[0005] The patent with publication number CN 117117211 A published on November 24, 2023 discloses a hydrogen fuel cell catalyst and preparation method of graphene oxide wrapped Pt-SnS, wherein the catalyst is spherical, and the catalyst uses sulfonated graphene oxide as a carrier, and the sulfonated graphene oxide has a spherical mesh structure, and Pt-SnS is grafted on the sulfonated graphene oxide carrier, and Pt-SnS is coated inside the spherical mesh carrier. The sulfonated graphene oxide in the catalyst forms a sphere to wrap around the reaction active site, thereby improving the catalytic stability of the Pt nanoparticles; after high-temperature reduction, a Pt-SnS alloy is formed in situ on Pt, and SnS can change the d-band central potential in Pt, thereby changing the electron distribution on the Pt surface, which is beneficial to the adsorption of oxygen-containing functional groups by the active site, thereby improving the catalytic efficiency of the catalyst. However, its preparation method is complicated and does not solve the problem of electrochemical corrosion. Summary of the invention

[0006] The purpose of the present invention is to provide a graphene-doped carbon carrier platinum-carbon catalyst material and a preparation method thereof, wherein the carbon aerogel is prepared by a sol-gel method, has better electrochemical corrosion resistance, and the carbon aerogel material is modified by graphene to further improve the catalytic activity and stability of the Pt / C catalyst ORR. The preparation method of the present invention is simple, efficient, and suitable for industrial promotion.

[0007] Another object of the present invention is to provide an application of a graphene-doped carbon-supported platinum-carbon catalyst material in a hydrogen fuel cell. As the cathode and anode catalyst of the membrane electrode in the hydrogen fuel cell, the material has excellent catalytic performance, stable performance, and good corrosion resistance and durability.

[0008] The specific technical solutions of the present invention are as follows:

[0009] A method for preparing a graphene-doped carbon-supported platinum-carbon catalyst material comprises the following steps:

[0010] 1) dissolving resorcinol in a mixed solution of anhydrous ethanol and ultrapure water, adding concentrated hydrochloric acid and graphene slurry, heating and stirring in an oil bath under closed conditions, adding formaldehyde solution dropwise, after the raw materials are completely dissolved, heating the obtained mixed solution to react, obtaining an organic wet gel, and carbonizing it to obtain a graphene-doped carbon aerogel carrier material;

[0011] 2) The graphene-doped carbon aerogel carrier material is dispersed in ethylene glycol, and H is added dropwise to the obtained mixed solution under stirring. 2 PcqI 6 The solution was prepared, and an alkali solution was added to adjust the pH value to 12, and then microwave heating was performed for reaction. After freeze-drying, a graphene-doped carbon-supported platinum-carbon catalyst material was obtained.

[0012] In step 1), the amount ratio of resorcinol to the mixed solution of anhydrous ethanol and ultrapure water is 0.10-0.12 g / mL;

[0013] In step 1), the volume ratio of anhydrous ethanol to ultrapure water is 1:1;

[0014] In step 1), the mass fraction of the concentrated hydrochloric acid is 37%;

[0015] In step 1), the graphene slurry, the graphene slurry solvent is water, and the mass concentration of graphene in the graphene slurry is 5%;

[0016] In step 1), the volume ratio of the mixed solution of concentrated hydrochloric acid, anhydrous ethanol and ultrapure water is 1:20;

[0017] In step 1), the amount of graphene slurry is 10% to 40% of the mass of resorcinol;

[0018] In step 1), the mass fraction of the formaldehyde solution is 37%;

[0019] In step 1), the molar ratio of resorcinol to formaldehyde in the formaldehyde solution is n R :n F =1 / 2~1 / 3:1;

[0020] In step 1), the mixture is heated and stirred in an oil bath under closed conditions at a temperature of 55-80° C., and the mixture is stirred until the raw materials are completely dissolved.

[0021] In step 1), the heating reaction is carried out by heating in an oil bath at a temperature of 55-80°C for 6-12 hours; preferably at 75°C for 12 hours;

[0022] In step 1), the prepared organic wet gel is first cooled to room temperature, washed with water by centrifugation for 3-5 times, dried in a vacuum drying oven at 80° C. for 12 h, and then carbonized;

[0023] In step 1), the carbonization treatment conditions are: in an argon atmosphere, in a tube furnace, at 5°C min -1 The heating rate is from 650 to 850°C to the carbonization temperature, and the treatment time is from 3 to 5 hours.

[0024] The graphene-doped carbon aerogel carrier material prepared in step 1) is a mesoporous material, labeled as GO-CA, with a pore size of 3-4 nm, and the pore size is small and uniform.

[0025] In step 2), the ratio of graphene-doped carbon aerogel carrier material to ethylene glycol is 0.7-0.8 mg / mL;

[0026] In step 2), the H 2 PcqI 6 The volume ratio of the solution to ethylene glycol is 1:20, and the H 2 PcqI 6 The concentration of the solution is Pt content 10 mg / mL;

[0027] In step 2), the alkali solution is a 1.0 M sodium hydroxide aqueous solution, and the pH value of the mixed system is adjusted to 12.

[0028] In step 2), the microwave heating reaction is carried out at a temperature of 170° C. and a reaction time of 5 min;

[0029] In step 2), after the reaction is completed, the final product is collected by centrifugation, washed with deionized water for 3-5 times, and then dried in a freeze dryer to obtain a graphene-doped carbon aerogel carrier material, which is labeled as GO-CA-Pt catalyst material.

[0030] The stirring speed of the present invention is 300-500 r / min;

[0031] The present invention provides a graphene-doped carbon-supported platinum-carbon catalyst material, which is prepared by the above method. The product SEM image shows that it has an obvious petal-like structure and a multilayer structure, which effectively increases the specific surface area, that is, increases the exposure of the active sites.

[0032] The present invention provides an application of a graphene-doped carbon-supported platinum-carbon catalyst material in a hydrogen fuel cell as a cathode and anode catalyst of a membrane electrode in a hydrogen fuel cell. The specific application method is as follows:

[0033] S1. Disperse the GO-CA-Pt catalyst material in deionized water for full wetting, then add an alcohol system solvent and Nafion solution, and obtain a catalyst slurry by shearing;

[0034] S2. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry onto both sides of the proton exchange membrane. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110kPa, slurry flow rate 5mL / min, step width 8mm, nozzle height 30mm, nozzle travel speed 150mm / min; the effective working area of ​​the obtained CCM is 5cm×5cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05mg / cm respectively. 2 .

[0035] Before assembling a single cell, prepare the end plates, insulating plates, current collectors, carbon plates (single serpentine flow channel), CCM, carbon paper, gaskets, bolts, torque wrenches and other components and installation tools. The torque used when assembling a single cell is 4 N·m. Before testing a single cell, check the air tightness of the battery to ensure that there is no gas leakage.

[0036] The fuel cell test system is a Ningbo Beit single cell test bench, using a 25cm 2 The membrane electrode test is performed using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture is controlled by electric heating, thereby adjusting the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions are as follows: H 2 The stoichiometric ratio of / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 min before the polarization curve test, and the cumulative activation was 120 min.

[0037] In step S1, the mass ratio of GO-CA-Pt catalyst material, deionized water, alcohol system solvent and Nafion solution is 100:15:20:0.6; the alcohol system solvent used is anhydrous ethanol, isopropanol or isobutanol; when preparing the catalyst slurry, the water in the ultrasonic cleaning machine is kept in an ice water bath state.

[0038] At present, Pt / C catalysts have poor durability and stability. In the actual operating environment of fuel cells, platinum-based catalysts will partially dissolve, oxidize and aggregate as the oxygen reduction reaction proceeds, causing the ability to catalyze oxygen reduction to gradually decrease until the reaction cannot be accelerated. The present invention uses a carbon aerogel material with good electrochemical stability prepared by high-temperature carbonization as a catalyst carrier, and modifies the carbon aerogel material with graphene to further improve the catalytic activity and stability of the Pt / C catalyst ORR.

[0039] Compared with the prior art, the present invention uses a carbon aerogel material with good electrochemical stability prepared by high-temperature carbonization as a catalyst carrier, specifically using a sol-gel method to prepare carbon aerogel (CA). CA has a higher degree of graphitization than commercial carbon black, so under extremely high potential conditions, CA has better electrochemical corrosion resistance. Platinum nanoparticles are loaded on CA, and the prepared Pt / CA has high catalytic activity and better ORR long-term cycle stability. The results show that the carbon aerogel (CA) prepared by the sol-gel method is an excellent Pt-based catalyst carrier. At the same time, the present invention modifies the carbon aerogel material by graphene to further improve the catalytic activity and stability of the Pt / C catalyst ORR. After graphene is doped with carbon aerogel, it transitions from a single-level structure to a hierarchical structure, and the presence of graphene inhibits its shrinkage, resulting in a portion of carbon aerogel nanoparticles attached to the graphene surface during the carbonization process, and the other part is distributed in the gaps of the graphene sheet in the form of microparticles. Therefore, the doped aerogel forms a unique hierarchical micro-nanostructure. The close bonding and synergistic coupling effect between graphene and the nanoparticles loaded thereon make the graphene-based composite material have higher oxygen reduction catalytic activity and catalyst carrier stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the scanning electron microscope image of GO-CA2 material;

[0041] Figure 2 Polarization curves of CA-Pt and GO-CA2-Pt. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0044] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0045] The graphene slurry used in the present invention has water as solvent, and the mass concentration of graphene in the graphene slurry is 5%.

[0046] Example 1 (for comparison)

[0047] A method for preparing a graphene-doped carbon carrier catalyst material comprises the following steps:

[0048] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇) =1:1), add 5 mL of concentrated hydrochloric acid (wt, 37%), stir at 25°C under closed conditions for 1 h until the reactants are completely dissolved, add 15 mL of formaldehyde solution (wt, 37%) dropwise to the solution under stirring at 300 r / min with an oil bath temperature of 75°C. After the raw materials are completely dissolved, keep the oil bath temperature at 75°C for 12 h to obtain an organic wet gel, which is then dried and cooled to room temperature, centrifuged and washed with water for 3 times, and dried in a vacuum drying oven at 80°C for 12 h. Then, the obtained material is placed in a tubular furnace and heated at 5°C min in an argon atmosphere. -1 The carbon aerogel / carbon carrier (CA) material can be obtained by heating the material at a carbonization temperature of 750 °C and a carbonization time of 5 h.

[0049] 2) Disperse 150 mg of the CA material obtained in step 1) uniformly in 200 mL of ethylene glycol by ultrasonic treatment to obtain a mixture; 2 PcqI 6 Solution (10 mg Pt mL -1 ) was added dropwise to the mixture under vigorous stirring; the pH value of the mixed system was adjusted to 12 with a 1.0M sodium hydroxide aqueous solution; then, the reaction solution was rapidly heated to 170°C by microwave and heated at this temperature for 5 minutes. The final product was collected by centrifugation, washed with deionized water 3 times, and dried in a freeze dryer to obtain a CA-Pt catalyst material.

[0050] An application of a graphene-doped carbon carrier catalyst material in a hydrogen fuel cell, specifically:

[0051] Take 100 mg of the catalyst material obtained in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then disperse at high speed shear for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice water bath state of 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of ​​the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .

[0052] Use 25cm 2 The membrane electrode test is performed using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture is controlled by electric heating, thereby adjusting the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions are as follows: H 2 The stoichiometric ratio of / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 min before the polarization curve test, and the cumulative activation was 120 min.

[0053] Example 2

[0054] A method for preparing a graphene-doped carbon-supported platinum-carbon catalyst material comprises the following steps:

[0055] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇) =1:1), 5 mL of concentrated hydrochloric acid (wt, 37%) and 1.1 g of graphene slurry were added to the mixed solution, and stirred at 25°C under closed conditions for 1 h until the reactants were completely dissolved. Under the conditions of stirring with a stirrer at 300 r / min and an oil bath temperature of 75°C, 15 mL of formaldehyde solution (wt, 37%) was added dropwise to the solution. After the raw materials were completely dissolved, the oil bath temperature was maintained at 75°C for 12 h to obtain an organic wet gel, which was dried and cooled to room temperature, centrifuged and washed with water 3 times, and dried in a vacuum drying oven at 80°C for 12 h. The obtained material was then placed in a tubular furnace and heated at 5°C min in an argon atmosphere. -1 The heating rate is 0.0447 W, the carbonization temperature is 750 °C, and the carbonization time is 5 h, then the graphene-doped carbon aerogel / carbon carrier (GO-CA1) material can be obtained.

[0056] 2) 150 mg of GO-CA1 prepared in step 1) was evenly dispersed in 200 mL of ethylene glycol by ultrasonic treatment. 2 PcqI 6 Solution (10 mg Pt mL -1 ) was added dropwise to the mixture under vigorous stirring. The pH value of the mixture was adjusted to 12 with sodium hydroxide aqueous solution (1.0 M). Then, the reaction solution was quickly heated to 170°C and heated at this temperature for 5 minutes. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain GO-CA1-Pt catalyst material.

[0057] Application of a graphene-doped carbon-supported platinum-carbon catalyst material in hydrogen fuel cells:

[0058] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of ​​the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .

[0059] Use 25cm 2 The membrane electrode test is performed using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture is controlled by electric heating, thereby adjusting the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions are as follows: H 2 The stoichiometric ratio of / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 min before the polarization curve test, and the cumulative activation was 120 min.

[0060] Example 3

[0061] A method for preparing a graphene-doped carbon-supported platinum-carbon catalyst material comprises the following steps:

[0062] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇)=1:1), 5 mL of concentrated hydrochloric acid (wt, 37%) and 2.2 g of graphene slurry were added to the mixed solution, and stirred at 25°C under closed conditions for 1 h until the reactants were completely dissolved. Under the conditions of stirring with a stirrer at 300 r / min and an oil bath temperature of 75°C, 15 mL of formaldehyde solution (wt, 37%) was added dropwise to the solution. After the raw materials were completely dissolved, the oil bath temperature was maintained at 75°C for 12 h to obtain an organic wet gel, which was dried and cooled to room temperature, centrifuged and washed with water 3 times, and dried in a vacuum drying oven at 80°C for 12 h. The obtained material was then placed in a tubular furnace and heated at 5°C min in an argon atmosphere. -1 The heating rate is 0.0447 W, the carbonization temperature is 750 °C, and the carbonization time is 5 h, then the graphene-doped carbon aerogel / carbon carrier (GO-CA2) material can be obtained.

[0063] 2) 150 mg of GO-CA2 material prepared in step 1) was evenly dispersed in 200 mL of ethylene glycol by ultrasonic treatment. 2 PcqI 6 Solution (10 mg Pt mL -1 ) was added dropwise to the mixture under vigorous stirring. The pH value of the mixture was adjusted to 12 with sodium hydroxide aqueous solution (1.0 M). Then, the reaction solution was quickly heated to 170°C and heated at this temperature for 5 minutes. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain GO-CA2-Pt catalyst material.

[0064] Application of a graphene-doped carbon-supported platinum-carbon catalyst material in hydrogen fuel cells:

[0065] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of ​​the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .

[0066] Use 25cm 2The membrane electrode test is performed using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture is controlled by electric heating, thereby adjusting the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions are as follows: H 2 The stoichiometric ratio of / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 min before the polarization curve test, and the cumulative activation was 120 min.

[0067] Figure 1 This is a scanning electron microscope image of the GO-CA2 material. It can be seen from the image that some carbon aerogel particles are attached to the surface of the petal-shaped graphene, while some exist independently, forming two hierarchical structures.

[0068] Figure 2 The polarization curves of CA-Pt and GO-CA2-Pt are shown in Figure 2. The polarization performance test results are better than those of carbon supports not modified with graphene, indicating that the catalyst has more exposed active sites, high activity, and no agglomeration.

[0069] The electrochemical test results show that the performance improvement effect is obvious. The chronoamperometric curve recorded at a constant voltage of 1.2V shows that GO-CA shows a lower corrosion current value during the entire test, which is lower than that of the unmodified carbon aerogel CA, showing better anti-electrochemical corrosion performance. Accelerated durability testing (ADT) was performed with 15,000 cycles in the voltage range of 0.6-1.0V. All CV curves show a broad hydrogen adsorption peak in the low potential range. For the GO-CA2-Pt catalyst, the polarization performance reaches 0.656V@2000mA / cm 2 .

[0070] Example 4

[0071] A method for preparing a graphene-doped carbon-supported platinum-carbon catalyst material comprises the following steps:

[0072] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇) =1:1), 5 mL of concentrated hydrochloric acid (wt, 37%) and 3.5 g of graphene slurry were added to the mixed solution, and stirred at 25°C under closed conditions for 1 h until the reactants were completely dissolved. Under the conditions of stirring with a stirrer at 300 r / min and an oil bath temperature of 75°C, 15 mL of formaldehyde solution (wt, 37%) was added dropwise to the solution. After the raw materials were completely dissolved, the oil bath temperature was maintained at 75°C for 12 h to obtain an organic wet gel, which was dried and cooled to room temperature, centrifuged and washed with water 3 times, and dried in a vacuum drying oven at 80°C for 12 h. The obtained material was then placed in a tubular furnace and heated at 5°C min in an argon atmosphere. -1The heating rate is 0.0447 W, the carbonization temperature is 750 °C, and the carbonization time is 5 h, then the graphene-doped carbon aerogel / carbon carrier (GO-CA3) material can be obtained.

[0073] 2) 150 mg of GO-CA3 material prepared in step 1) was evenly dispersed in 200 mL of ethylene glycol by ultrasonic treatment. 2 PcqI 6 Solution (10 mg Pt mL -1 ) was added dropwise to the mixture under vigorous stirring. The pH value of the mixture was adjusted to 12 with sodium hydroxide aqueous solution (1.0 M). Then, the reaction solution was quickly heated to 170°C and heated at this temperature for 5 minutes. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain GO-CA3-Pt catalyst material.

[0074] Application of a graphene-doped carbon-supported platinum-carbon catalyst material in hydrogen fuel cells:

[0075] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of ​​the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .

[0076] Use 25cm 2 The membrane electrode test is performed using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture is controlled by electric heating, thereby adjusting the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions are as follows: H 2 The stoichiometric ratio of / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 min before the polarization curve test, and the cumulative activation was 120 min.

[0077] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a graphene-doped carbon-supported platinum-carbon catalyst material, characterized in that: The preparation method comprises the following steps: 1) Dissolve resorcinol in a mixed solution of anhydrous ethanol and ultrapure water, then add concentrated hydrochloric acid and graphene slurry, heat and stir in an oil bath under closed conditions, add formaldehyde solution dropwise, and after the raw materials are completely dissolved, heat the obtained mixed solution to react to obtain an organic wet gel, and then perform carbonization treatment to obtain a graphene-doped carbon aerogel carrier material; 2) The graphene-doped carbon aerogel carrier material is dispersed in ethylene glycol, and H2PtCl6 solution is added dropwise to the obtained mixed solution under stirring, and then an alkali solution is added to adjust the pH value to 12, and then microwave heating is performed for reaction, and freeze-drying is performed to obtain a graphene-doped carbon carrier platinum-carbon catalyst material; In step 1), the volume ratio of anhydrous ethanol to ultrapure water is 1:1; the heating reaction has a reaction temperature of 55-80°C and a reaction time of 6-12 hours.

2. The preparation method according to claim 1, characterized in that: In step 1), the amount of the graphene slurry is 10% to 40% of the mass of resorcinol.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1), the molar ratio of resorcinol to formaldehyde in the formaldehyde solution is n R :n F =1 / 2~1 / 3:

1.

4. The preparation method according to claim 1, characterized in that: In step 1), the carbonization treatment conditions are: heating to 650-850° C. in an argon atmosphere, and the treatment time is 3-5 h.

5. The preparation method according to claim 1, characterized in that: In step 2), the amount ratio of graphene-doped carbon aerogel carrier material to ethylene glycol is 0.7-0.8 mg / mL; the volume ratio of the H2PtCl6 solution to ethylene glycol is 1:20, and the concentration of the H2PtCl6 solution is a Pt content of 10 mg / mL.

6. The preparation method according to claim 1 or 5, characterized in that: In step 2), the microwave heating reaction is carried out at a temperature of 170° C. and a reaction time of 5 min.

7. A graphene-doped carbon-supported platinum-carbon catalyst material prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the graphene-doped carbon-supported platinum-carbon catalyst material according to claim 7 in a hydrogen fuel cell.