High silicon-containing core-shell acrylic emulsion and preparation method thereof
Through the preparation method of high-silicon core-shell acrylate emulsion, the redox system and non-ionic emulsifier are used to avoid hydrolysis and polycondensation, which solves the problem of poor bonding performance of water-based sealants to glass and metal substrates, and realizes the emulsion Improved stability and adhesion.
Patent Information
- Application Number
- CN202410351172.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-26
AI Technical Summary
The existing water-based sealants have poor adhesive properties on glass, metal and other substrates, and the silanyloxy groups and silanylhydroxy groups are prone to hydrolysis and polycondensation during use, resulting in a decrease in activity.
The preparation method of high-silicon core-shell acrylate emulsion is adopted to avoid hydrolysis and polycondensation through redox system initiators and non-ionic emulsifiers, and the conversion rate is improved by using persulfate initiators to ensure the stability of silanyloxy groups and silanoxy groups. and adhesiveness.
Effectively retain and utilize the alkoxy groups and silicon hydroxy groups in the emulsion, improving the adhesion and stability of the emulsion to the substrate and improving the adhesion to glass.
Smart Images

Figure CN118146462B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resin or emulsion preparation, and particularly relates to a high-silicon-containing core-shell acrylic emulsion and a preparation method thereof. Background Art
[0002] Water-based polymer emulsions not only have the characteristics of chemical stability, weather resistance, light resistance, and chemical resistance, but also have the characteristics of corrosion resistance, acid and alkali resistance, good water film formation, good color retention, no pollution, good process stability, and safe application. Water-based sealants based on polymer emulsions are gaining more and more attention, but the poor bonding performance of water-based sealants to glass, metal and other substrates has become a factor restricting the development of water-based sealants.
[0003] In order to effectively enhance the adhesion of water-based sealants to substrates such as glass and metal, a polyacrylic acid emulsion is usually obtained by modifying the acrylate emulsion with functional monomers. Although the product failure caused by the thickening of the system is alleviated to a certain extent, the thickening and agglomeration of the glue will still occur. The prior art modifies the acrylate emulsion with silicone, and achieves thermal stability and low surface free energy by controlling the content of polysiloxane, but during use, it will cause the alkoxy groups that are effective for glass to rapidly hydrolyze and self-condense, resulting in reduced activity. Therefore, it is necessary to develop a high-silicon core-shell acrylate emulsion and a preparation method thereof to solve the problem that the existing emulsion system has low content of uncrosslinked silanoxy groups and silanol groups, so that the silanoxy groups and silanol groups can form bonds with the surface of the substrate after the emulsion contacts the bonded substrate, thereby improving the adhesion of the emulsion. Summary of the invention
[0004] The present invention provides a high silicon-containing core-shell acrylic emulsion and a preparation method thereof. The initiators during the polymerization of the core layer, namely, reducing agent 1 and oxidizing agent 1, are redox system initiators, and the emulsifier is a non-ionic emulsifier, so as to avoid the hydrolysis and polycondensation of alkoxy groups caused by the generation of hydrogen ions by heating or hydrolysis of persulfate and ionic emulsifier. Similarly, the redox system of the first shell layer and the non-ionic initiators, oxidizing agent 2 and reducing agent 2, can avoid the polycondensation of silanol groups formed by hydrolysis in the catalytic latex particles and encapsulate them inside, so that the prepared emulsion is more stable. The encapsulation of the first shell layer can protect the silanol groups and silanol groups of the inner layer. The use of persulfate initiator during the preparation of the second shell layer can improve the conversion rate, and the monomers in the system are fully reacted, so that the reaction is more complete.
[0005] The technical solution of the present invention is:
[0006] In a first aspect, a method for preparing a high silicon-containing core-shell acrylic emulsion is disclosed, comprising the following steps:
[0007] 1) Preparation of nuclear pre-emulsion: Add acrylate monomer 1, emulsifier 1 and deionized water into a reaction tank 1, homogenize and emulsify, and set aside; the mass ratio of acrylate monomer 1, emulsifier 1 and deionized water is 40-60:1-3:40-60.
[0008] 2) Preparation of shell pre-emulsion 1: Add acrylate monomer 2, emulsifier 2 and deionized water into reaction tank 2, homogenize and emulsify, and set aside; the mass ratio of acrylate monomer 2, emulsifier 2 and deionized water is 50-80:1-3:40-60.
[0009] 3) Preparation of shell pre-emulsion 2: Add acrylate monomer 3, emulsifier 3, pH buffer 1 and deionized water into reaction tank 3, homogenize and emulsify, and set aside; the mass ratio of acrylate monomer 3, emulsifier 3, pH buffer 1 and deionized water is 80-100:0.5-3:0.1-1:60-120.
[0010] 4) Preparation of core layer: add emulsifier 4, pH buffer 2, deionized water and reducing agent 1 into the reactor, increase the temperature during stirring, and simultaneously add the core pre-emulsion, coupling agent and oxidant 1 dropwise, the core pre-emulsion is added dropwise within 20-40 minutes, and stirred at a constant temperature after addition; the mass ratio of emulsifier 4, pH buffer 2, deionized water, reducing agent 1, coupling agent and oxidant 1 is 2-10:0.1-0.5:60-100:0.05-0.4:20-30:0.05-0.5.
[0011] 5) Preparation of the first shell layer: Add reducing agent 2 to the core layer emulsion obtained in step 4), dropwise add shell pre-emulsion 1 and oxidant 2, and stir at a constant temperature after the dropwise addition. The mass ratio of reducing agent 2 to oxidant 2 is 0.1-1:1-3.
[0012] 6) Preparation of the second shell layer: heating to 65-80°C, adding a molecular weight regulator, dropping the shell pre-emulsion 2 and the initiator into the system for 2-4 hours, keeping warm for 1 hour, adding ethylenediaminetetraacetic acid (EDTA) to precipitate ferrous ions; cooling to 50-60°C, adding a neutralizer, neutralizing to a pH of 7-8, filtering to obtain the target product, a high silicon-containing core-shell acrylic emulsion; the mass ratio of the molecular weight regulator, the initiator, and the EDTA is 0.5-2:0.5-2:0.1-1.
[0013] Preferably, the acrylate monomer 1, acrylate monomer 2 and acrylate monomer 3 are one or more of lauryl acrylate, isobutyl acrylate, isotridecyl acrylate, methoxypolyethylene glycol methacrylate, acrylic acid, butyl acrylate, methyl methacrylate, hydroxyethyl acrylate, α-methacrylic acid and isooctyl acrylate, and more preferably a mixture of acrylic acid, butyl acrylate, methyl methacrylate, hydroxyethyl acrylate, α-methacrylic acid and isooctyl acrylate.
[0014] Preferably, the emulsifier one, the emulsifier two and the emulsifier four are all octylphenol polyoxyethylene ether 10 (OP-10), multi-branched isomeric tridecanol polyoxyethylene ether 30 (OXO-1330), sorbitan oleate (Span-80), polysorbate 80 (Tween-80), polysorbate 85 (Tween-85), polysorbate 20 (Tween-20), polyoxyethylene lauryl ether (Brij-35), polyethylene glycol stearate (Myrj-53), fatty alcohol polyoxyethylene ether 9 (AEO-9), fatty alcohol polyoxyethylene ether 7 (AEO-7) Any two or more of the composite, preferably OP-10, OXO-1330 composite emulsifier, the mass ratio of the two is 1:3; the emulsifier three is octylphenol polyoxyethylene Any two or more of the following composite emulsifiers: OP-10, OXO-1330, Sorbitan Oleate (Span-80), Tween-80, Tween-85, Tween-20, Brij-35, Myrj-53, AEO-9, AEO-7, SDS, SDBS, AEC-9Na, and potassium lauryl phosphate, more preferably sodium lauryl sulfate and OP-10 composite emulsifier, with a mass ratio of 1:2.
[0015] Preferably, pH buffer agent 1 and pH buffer agent 2 are both one of sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, sodium bicarbonate, and potassium bicarbonate, and more preferably sodium bicarbonate.
[0016] Preferably, the reducing agent 1 is one of tetraethylenepentamine, pentaethylenehexamine, N-monoalkylethylenediamine, triaminoethylamine, and triethylenetetramine, preferably tetraethylenepentamine; the reducing agent 2 is ferrous pyrophosphate or ferrous sulfate, more preferably ferrous pyrophosphate.
[0017] Preferably, the homogenization and emulsification time in steps 1), 2) and 3) is 5-30 minutes; the temperature in the preparation of the core layer emulsion in step 4) is raised to 25-50°C, more preferably 40°C; the constant temperature stirring time in steps 4) and 5) is 0.5-2 hours.
[0018] Preferably, in the step 4), the coupling agent is one or more of vinyl trimethoxy silane, γ-methacryloxypropyl trimethoxy silane, γ-methacryloxypropyl triethoxy silane, γ-methacryloxypropyl methyl dimethoxy silane, and γ-methacryloxypropyl triisopropoxy silane, and more preferably a mixture of vinyl trimethoxy silane, γ-methacryloxypropyl triethoxy silane, and γ-methacryloxypropyl triisopropoxy silane, with a mass ratio of 1:1:2.
[0019] Preferably, the oxidant one and the oxidant two are one of cumene hydroperoxide, hydrogen peroxide, benzoyl peroxide and potassium chromate.
[0020] Preferably, the molecular weight regulator is one of n-dodecyl mercaptan and succinic acid mono-n-dodecyl mercaptan ester, preferably n-dodecyl mercaptan; the neutralizer is one or more of sodium hydroxide, ammonia water, triethylamine, and sodium carbonate, more preferably triethylamine; the initiator is one of potassium persulfate, sodium persulfate, and ammonium persulfate.
[0021] In a second aspect, a high silicon-containing core-shell acrylic emulsion prepared by the preparation method is disclosed.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention effectively retains the alkoxy and silanol groups in the emulsion and provides a preparation method thereof, which is scientific, reasonable, simple and easy to implement.
[0024] 2. The initiators during the polymerization of the core layer, namely the reducing agent 1 and the oxidizing agent 1, are redox system initiators, and the emulsifier is a non-ionic emulsifier, which prevents persulfate and ionic emulsifiers from generating hydrogen ions when heated or hydrolyzed, thereby causing hydrolysis and polycondensation of alkoxy groups. Similarly, the redox system of the first shell layer and the non-ionic initiators, the oxidizing agent 2 and the reducing agent 2, can avoid the polycondensation of silanol groups formed by hydrolysis in the catalytic latex particles and encapsulate them inside, making the prepared emulsion more stable. The encapsulation of the first shell layer can protect the silanol groups and silanol groups of the inner layer. The use of persulfate initiators in the preparation of the second shell layer can increase the conversion rate, complete the reaction of the monomers in the system, and make the reaction more complete. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the infrared spectra of Example 1 of the present invention and Comparative Example 1.
[0026] Figure 2 It is a comparison diagram of glass bonding between Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment provides a method for preparing a high silicon-containing core-shell acrylic emulsion, comprising the following steps:
[0030] 1) Preparation of nuclear pre-emulsion: 20 g butyl acrylate, 15 g methyl methacrylate, 12 g isooctyl acrylate, 42 g deionized water, 0.3 g OP-10, and 0.9 g OXO-1330 were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0031] 2) Preparation of shell pre-emulsion 1: 30 g methyl methacrylate, 10 g isotridecyl acrylate, 20 g butyl acrylate, 0.4 g OP-10, 1.2 g OXO-1330 were mixed with 63 g deionized water, and emulsified in a homogenizer for 10 min; set aside;
[0032] 3) Preparation of shell pre-emulsion 2: 42 g of lauryl acrylate, 26.5 g of butyl acrylate, 26.5 g of methyl methacrylate, 1 g of acrylic acid, 0.75 g of hydroxyethyl acrylate, 0.5 g of sodium lauryl sulfate, 1 g of OP-10, 0.7 g of sodium bicarbonate, and 75 g of deionized water were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0033] 4) Preparation of core layer: 0.8g OP-10, 2.4g OXO-1330, 0.1g tetraethylenepentamine, 0.2g sodium bicarbonate, 75g deionized water were added to a four-necked flask equipped with a condenser, a stirrer and a thermometer, and the temperature was raised to 40°C during stirring. At the same time, the core pre-emulsion prepared in step 1), 6g vinyl trimethoxysilane, 6g γ-methacryloxypropyl triethoxysilane, 12g γ-methacryloxypropyl triisopropoxysilane, and 0.12g cumene hydroperoxide were dripped within 30min, and stirred at a constant temperature for 1h after dripping;
[0034] 5) Preparation of the first shell layer: 0.7 g of ferrous pyrophosphate was added to the system, and at the same time, the first shell layer pre-emulsion prepared in step 2) and 1.4 g of cumene hydroperoxide were added dropwise, and after the addition was completed, the mixture was stirred at a constant temperature for 1 hour;
[0035] 6) Preparation of the second shell layer: the temperature was raised to 77°C, 0.5 g of n-dodecyl mercaptan was added, and the second shell layer pre-emulsion and 0.5 g of potassium persulfate were added to the system by a Lange peristaltic pump, the addition time was 2 h, and the temperature was kept for 1 h. 0.6 g of EDTA was added to precipitate ferrous ions; after keeping the temperature for 2 h, the heating was turned off, the temperature was lowered to 55°C, neutralized, and triethylamine was used to neutralize to a pH of 7.4. After completion, the target product, a high silicon-containing core-shell acrylic emulsion, was obtained by filtering with a filter. Its infrared chromatogram is shown as follows: Figure 1 shown.
[0036] Comparative Example 1
[0037] Preparation of ordinary silicone-acrylic emulsion: prepare pre-emulsion with 52g butyl acrylate, 45g methacrylic acid, 1g methacrylic acid, 0.3g sodium dodecyl sulfate, 0.5g OP-10 and 60g water; dissolve 0.3g ammonium persulfate in 10g water; add 60g water, 0.3g sodium dodecyl sulfate, 0.5g OP-10 and 0.5g sodium bicarbonate in a flask and heat to 75°C; add 10g pre-emulsion and 1g ammonium persulfate aqueous solution in the flask, and add pre-emulsion, ammonium persulfate aqueous solution and 7g vinyltrimethoxysilane at the same time after blue light appears in the flask; after the addition is completed, heat to 85°C and keep warm for 1h, neutralize the emulsion with ammonia water to pH 7-8, and filter to obtain silicone-acrylic emulsion. Its infrared chromatogram is shown as follows Figure 1 As shown, from Figure 1 It can be seen that at 1100cm -1 Up to 1200cm -1 The common silicone acrylic emulsion has multiple peaks, which proves the crosslinking of the coupling agent, while the single peak of the high silicon-containing core-shell acrylic emulsion prepared in Example 1 at the same wave number proves the existence of alkoxy groups. This shows that this preparation method successfully prepared a high silicon-containing acrylic emulsion and successfully retained the alkoxy groups.
[0038] The high silicon-containing core-shell acrylic emulsion prepared in Example 1 and the ordinary silicone acrylic emulsion in Comparative Example 1 were tested for glass bonding performance. The specific method is as follows: 200g of the emulsion was taken, 220g of 1250 mesh calcium carbonate was added to the emulsion, and the mixture was dispersed and then vacuum degassed and coated on the glass. Figure 2 As shown, Figure 2(a) represents the common silicone acrylic emulsion of comparative example 1, and (b) represents the high silicon-containing core-shell acrylic emulsion of example 1. It can be seen from the figure that the common silicone acrylic emulsion can be peeled off from the glass surface smoothly, proving that Si-OR has been almost completely cross-linked during the preparation process, while the adhesion formed between the emulsion prepared by the preparation method and the glass proves that the presence of Si-OR forms a chemical bond with the glass surface, thereby enhancing the adhesion and thus improving the stability of the emulsion.
[0039] Example 2
[0040] This embodiment provides a method for preparing a high silicon-containing core-shell acrylic emulsion, comprising the following steps:
[0041] 1) Preparation of nuclear pre-emulsion: 15 g butyl acrylate, 15 g methyl methacrylate, 18 g isooctyl acrylate, 42 g deionized water, 0.3 g OP-10, and 0.9 g OXO-1330 were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0042] 2) Preparation of shell pre-emulsion 1: 30 g methyl methacrylate, 10 g isotridecyl acrylate, 20 g butyl acrylate, 0.4 g OP-10, 1.2 g OXO-1330 were mixed with 63 g deionized water, and emulsified in a homogenizer for 10 min; set aside;
[0043] 3) Preparation of shell pre-emulsion 2: 40 g of lauryl acrylate, 26 g of butyl acrylate, 26 g of methyl methacrylate, 1 g of acrylic acid, 0.75 g of hydroxyethyl acrylate, 0.5 g of sodium lauryl sulfate, 1 g of OP-10, 0.7 g of sodium bicarbonate, and 75 g of deionized water were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0044] 4) Preparation of core layer: 0.8g OP-10, 2.4g OXO-1330, 0.1g triethylenetetramine, 0.3g disodium hydrogen phosphate, 75g deionized water were added to a four-necked flask equipped with a condenser, a stirrer and a thermometer. The temperature was raised to 40°C during stirring. At the same time, core pre-emulsion, 4g vinyltrimethoxysilane, 8g γ-methacryloxypropyltriethoxysilane, 15g γ-methacryloxypropyltriisopropoxysilane, and 0.15g cumene hydroperoxide were added dropwise within 30min. After the addition, the mixture was stirred at a constant temperature for 1h.
[0045] 5) Preparation of the first shell layer: Add 0.7 g of ferrous pyrophosphate to the system, and simultaneously drop the first shell layer pre-emulsion and 1.4 g of cumene hydroperoxide, and stir at a constant temperature for 1 h after the dropwise addition;
[0046] 6) Preparation of the second shell layer: the temperature was raised to 72°C, 0.5 g of n-dodecyl mercaptan was added, and the second shell layer pre-emulsion and 0.5 g of potassium persulfate were added to the system through a Lange peristaltic pump, the addition time was 2 h, and the mixture was kept warm for 1 h. 0.6 g of EDTA was added to precipitate ferrous ions. After keeping warm for 2 h, the heating was turned off, the temperature was lowered to 55°C, and neutralization was performed. The mixture was neutralized with triethylamine to a pH of 7.2. After completion, the target product, a high silicon-containing core-shell acrylic emulsion, was obtained by filtering with a filter.
[0047] Example 3
[0048] This embodiment provides a method for preparing a high silicon-containing core-shell acrylic emulsion, comprising the following steps:
[0049] 1) Preparation of nuclear pre-emulsion: 18 g isobutyl acrylate, 20 g methyl methacrylate, 18 g isooctyl acrylate, 45 g deionized water, 0.4 g Span-80, and 1 g OXO-1330 were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0050] 2) Preparation of shell pre-emulsion 1: 30 g methyl methacrylate, 10 g lauryl acrylate, 20 g butyl acrylate, 0.4 g Span-80, 0.8 g Brij-35 and 60 g deionized water were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0051] 3) Preparation of shell pre-emulsion 2: 40 g of lauryl acrylate, 26 g of butyl acrylate, 26 g of methyl methacrylate, 1 g of acrylic acid, 1.5 g of hydroxyethyl acrylate, 0.5 g of sodium lauryl sulfate, 1 g of OP-10, 0.5 g of sodium dihydrogen phosphate and 75 g of deionized water were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0052] 4) Preparation of core layer: 0.8 g Tween-80, 2.4 g OXO-1330, 0.13 g triethylenetetramine, 0.3 g sodium bicarbonate, and 75 g deionized water were added to a four-necked flask equipped with a condenser, a stirrer, and a thermometer. The temperature was raised to 40°C during stirring. At the same time, core pre-emulsion, 6 g vinyl trimethoxysilane, 7 g γ-methacryloxypropyl triethoxysilane, 15 g γ-methacryloxypropyl triisopropoxysilane, and 0.16 g cumene hydroperoxide were added dropwise within 30 min. After the addition, the mixture was stirred at a constant temperature for 1 h.
[0053] 5) Preparation of the first shell layer: Add 0.7 g of ferrous pyrophosphate to the system, and simultaneously drop the first shell layer pre-emulsion and 1.4 g of cumene hydroperoxide, and stir at a constant temperature for 1 h after the dropwise addition;
[0054] 6) Preparation of the second shell layer: the temperature was raised to 75°C, 0.5 g of n-dodecyl mercaptan was added, and the second shell layer pre-emulsion and 0.5 g of potassium persulfate were added to the system through a Lange peristaltic pump, the addition time was 2 h, and the mixture was kept warm for 1 h. 0.6 g of EDTA was added to precipitate ferrous ions. After keeping warm for 2 h, the heating was turned off, the temperature was lowered to 50°C, and neutralization was performed. The mixture was neutralized with triethylamine to a pH of 7.2. After completion, the target product, a high silicon-containing core-shell acrylic emulsion, was obtained by filtering with a filter.
[0055] Example 4
[0056] This embodiment provides a method for preparing a high silicon-containing core-shell acrylic emulsion, comprising the following steps:
[0057] 1) Preparation of nuclear pre-emulsion: 18 g butyl acrylate, 20 g methyl methacrylate, 19 g isotridecyl acrylate, 60 g deionized water, 0.4 g Span-80, and 1 g Myrj-53 were mixed, emulsified in a homogenizer for 13 min, and set aside;
[0058] 2) Preparation of shell pre-emulsion 1: 35 g methyl methacrylate, 12 g lauryl acrylate, 20 g isobutyl acrylate, 0.4 g AEO-7, 0.8 g Tween-85 were mixed with 60 g deionized water, emulsified with a homogenizer for 10 min, and set aside;
[0059] 3) Preparation of shell pre-emulsion 2: 40 g of lauryl acrylate, 26 g of butyl acrylate, 26 g of methyl methacrylate, 0.8 g of α-methacrylic acid, 0.5 g of AEC-9, 1 g of OP-10, 0.5 g of disodium hydrogen phosphate and 75 g of deionized water were mixed, emulsified in a homogenizer for 8 min, and set aside;
[0060] 4) Preparation of core layer: 0.8 g Tween-80, 2.4 g OXO-1330, 0.2 g triaminoethylamine, 0.2 g potassium bicarbonate and 80 g deionized water were added to a four-necked flask equipped with a condenser, a stirrer and a thermometer. The temperature was raised to 25°C during stirring. At the same time, core pre-emulsion, 6 g vinyl trimethoxysilane, 6 g γ-methacryloxypropyl triethoxysilane, 20 g vinyl trimethoxysilane, 6 g γ-methacryloxypropyl methyldimethoxysilane, 6 g γ-methacryloxypropyl triisopropoxysilane and 0.25 g cumene hydroperoxide were added dropwise within 45 min. After the addition, the mixture was stirred at a constant temperature for 1 h.
[0061] 5) Preparation of the first shell layer: Add 0.7 g of ferrous sulfate to the system, and simultaneously drop the first shell layer pre-emulsion and 1.4 g of cumene hydroperoxide, and stir at a constant temperature for 1 h after the dropwise addition;
[0062] 6) Preparation of the second shell layer: the temperature was raised to 75°C, 0.6 g of n-dodecyl mercaptan was added, and the second shell layer pre-emulsion and 0.5 g of potassium persulfate were added to the system through a Lange peristaltic pump, the addition time was 3 h, and the mixture was kept warm for 1 h. 0.9 g of EDTA was added to precipitate ferrous ions. After keeping warm for 1.5 h, the heating was turned off, the temperature was lowered to 54°C, and neutralization was performed. The mixture was neutralized with triethylamine to a pH of 7.6. After completion, the target product, a high silicon-containing core-shell acrylic emulsion, was obtained by filtering with a filter.
[0063] Example 5
[0064] This embodiment provides a method for preparing a high silicon-containing core-shell acrylic emulsion, comprising the following steps:
[0065] 1) Preparation of nuclear pre-emulsion: 18 g butyl acrylate, 20 g methyl methacrylate, 19 g isotridecyl acrylate, 2 g hydroxyethyl acrylate, 60 g deionized water, 0.4 g Span-80, and 1 g Brij-35 were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0066] 2) Preparation of shell pre-emulsion 1: 30 g methyl methacrylate, 15 g lauryl acrylate, 25 g isobutyl acrylate, 0.4 g Myrj-53, 0.8 g Tween-85, and 60 g deionized water were mixed, emulsified in a homogenizer for 10 min, and set aside;
[0067] 3) Preparation of shell pre-emulsion 2: 40 g of lauryl acrylate, 26 g of butyl acrylate, 26 g of methyl methacrylate, 0.5 g of sodium dodecylbenzene sulfonate, 1 g of OP-10, 0.8 g of dipotassium hydrogen phosphate and 75 g of deionized water were mixed, emulsified in a homogenizer for 15 min, and set aside;
[0068] 4) Preparation of core layer: 0.8 g Tween-80, 2.4 g OXO-1330, 0.15 g triaminoethylamine, 0.2 g sodium bicarbonate and 85 g deionized water were added to a four-necked flask equipped with a condenser, a stirrer and a thermometer. The temperature was raised to 30°C during stirring. At the same time, core pre-emulsion, 8 g vinyl trimethoxysilane, 8 g γ-methacryloxypropyl methyl dimethoxysilane, 14 g γ-methacryloxypropyl triisopropoxysilane and 0.35 g cumene hydroperoxide were added dropwise within 45 min. After the addition, the mixture was stirred at a constant temperature for 1 h.
[0069] 5) Preparation of the first shell layer: Add 0.7 g of ferrous sulfate to the system, and simultaneously drop the first shell layer pre-emulsion and 1.5 g of hydrogen peroxide, and stir at a constant temperature for 1 h after the dropwise addition;
[0070] 6) Preparation of the second shell layer: the temperature was raised to 75°C, 0.6 g of n-dodecyl mercaptan was added, and the second shell layer pre-emulsion and 0.5 g of potassium persulfate were added to the system through a Lange peristaltic pump, the addition time was 3 h, and the mixture was kept warm for 1 h. 0.9 g of EDTA was added to precipitate ferrous ions. After keeping warm for 2 h, the heating was turned off, the temperature was lowered to 50°C, neutralized, and neutralized with ammonia water to a pH of 7.6. After completion, the target product, a high silicon-containing core-shell acrylic emulsion, was obtained by filtering with a filter.
[0071] Although the present invention has been described in detail by combining the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing a high silicon-containing core-shell acrylic emulsion, characterized in that: The following steps are involved: 1) Preparation of nuclear pre-emulsion: Add acrylic acid ester monomer 1, emulsifier 1 and deionized water into reaction tank 1, homogenize and emulsify, and set aside; 2) Preparation of shell pre-emulsion 1: Add acrylate monomer 2, emulsifier 2 and deionized water into reaction tank 2, homogenize and emulsify, and set aside; 3) Preparation of shell pre-emulsion 2: Add acrylate monomer 3, emulsifier 3, pH buffer 1 and deionized water into reaction tank 3, homogenize and emulsify, and set aside; 4) Preparation of the core layer: Add emulsifier 4, pH buffer 2, deionized water and reducing agent 1 into the reactor, increase the temperature during stirring, and simultaneously drop the core pre-emulsion, coupling agent and oxidant 1, drop the core pre-emulsion within 20-40 minutes, and stir at a constant temperature after the drop is complete; 5) Preparation of the first shell layer: Add reducing agent 2 to the core layer emulsion obtained in step 4), dropwise add shell pre-emulsion 1 and oxidizing agent 2, and stir at a constant temperature after the dropwise addition is completed; 6) Preparation of the second shell layer: heating to 65-80°C, adding a molecular weight regulator, dropping the shell pre-emulsion 2 and the initiator into the system for 2-4 hours, keeping warm for 1 hour, adding ethylenediaminetetraacetic acid to precipitate ferrous ions; cooling to 50-60°C, adding a neutralizer, neutralizing to a pH of 7-8, filtering to obtain the target product, a high silicon-containing core-shell acrylate emulsion; The emulsifier 1, emulsifier 2 and emulsifier 4 are any two or more of octylphenol polyoxyethylene ether 10, multi-branched isomeric tridecanol polyoxyethylene ether 30, sorbitan oleate, polysorbate 80, polysorbate 85, polysorbate 20, polyoxyethylene lauryl ether, polyethylene glycol stearate, fatty alcohol polyoxyethylene ether 9, and fatty alcohol polyoxyethylene ether 7. The emulsifier 3 is any two or more of the composite emulsifiers selected from octylphenol polyoxyethylene ether 10, multi-branched isomeric tridecanol polyoxyethylene ether 30, sorbitan oleate, polysorbate 80, polysorbate 85, polysorbate 20, polyoxyethylene lauryl ether, polyethylene glycol stearate, fatty alcohol polyoxyethylene ether 9, fatty alcohol polyoxyethylene ether 7, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium fatty alcohol polyoxyethylene ether carboxylate, and potassium lauryl phosphate. The first reducing agent is one of tetraethylenepentamine, pentaethylenehexamine, N-monoalkylethylenediamine, triaminoethylamine, and triethylenetetramine, and the second reducing agent is ferrous pyrophosphate or ferrous sulfate; The oxidant 1 and the oxidant 2 are both one of cumene hydroperoxide, hydrogen peroxide and benzoyl peroxide; The acrylate monomer 1, acrylate monomer 2 and acrylate monomer 3 are one or more of lauryl acrylate, isobutyl acrylate, isotridecyl acrylate, methoxy polyethylene glycol methacrylate, acrylic acid, butyl acrylate, methyl methacrylate, hydroxyethyl acrylate, α-methacrylic acid and isooctyl acrylate; In the step 4), the coupling agent is one or more of vinyl trimethoxy silane, γ-methacryloxypropyl trimethoxy silane, γ-methacryloxypropyl triethoxy silane, γ-methacryloxypropyl methyl dimethoxy silane, and γ-methacryloxypropyl triisopropoxy silane.
2. The method for preparing the high silicon-containing core-shell acrylic emulsion according to claim 1, wherein: The pH buffer agent 1 and the pH buffer agent 2 are both one of sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, sodium bicarbonate, and potassium bicarbonate.
3. The method for preparing the high silicon-containing core-shell acrylic emulsion according to claim 1, characterized in that: The homogenization and emulsification time in steps 1), 2) and 3) is 5-30 minutes; the temperature in the preparation of the core layer in step 4) is raised to 25-50°C, and the constant temperature stirring time in steps 4) and 5) is 0.5-2 hours.
4. The method for preparing the high silicon-containing core-shell acrylic emulsion according to claim 1, wherein: The molecular weight regulator is one of n-dodecyl mercaptan and succinic acid mono-n-dodecyl mercaptan ester; the neutralizer is one or more of sodium hydroxide, ammonia water, triethylamine and sodium carbonate; and the initiator is one of potassium persulfate, sodium persulfate and ammonium persulfate.
5. A high silicon-containing core-shell acrylic emulsion prepared by the preparation method according to any one of claims 1 to 4.