A composite morphology of indium oxide nanomaterials and its application in VOC gas detection
By adjusting the ratio of urea and sodium dodecyl sulfonate in the preparation of indium oxide nanomaterials and using microwave treatment to form indium oxide nanomaterials with high dispersion cluster structures, the preparation method of indium oxide nanomaterials in the prior art is solved. The disadvantages of this achieve high sensitivity detection of VOC gas and feasibility of industrial production.
Patent Information
- Application Number
- CN202410310519.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-19
AI Technical Summary
The existing indium oxide nanomaterial preparation methods have problems such as harsh reaction conditions, high cost, difficulty in large-scale production, easy product agglomeration and low gas sensitivity performance, which limits its application effect in gas detection.
Based on the ordinary hydrothermal method, the ratio and dosage of urea, indium nitrate and sodium dodecyl sulfonate are adjusted, and microwave treatment is used to prepare indium oxide nanomaterial with high dispersion cluster structure, using urea as The alkali source and the surfactant sodium dodecyl sulfonate work together to control the crystal surface growth through microwave heating to form a composite morphological material with excellent gas sensitivity.
It realizes high sensitivity detection of VOC gas, especially good selectivity and sensitivity to formaldehyde, acetone, toluene and other gases. The microwave heating method saves energy, avoids agglomeration in traditional hydrothermal methods, and is suitable for industrial production.
Smart Images

Figure CN118164522B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses an indium oxide nano material with a composite morphology and application thereof in VOC gas detection, belonging to the technical field of nano materials. Background Art
[0002] Indium oxide (In 2 O 3 )The melting point, density and molecular weight are 2000℃, 7.19g / cm 3 , 277.63400, most of them are light yellow or white. In addition, its lattice energy is 13928 Kj / mo1. It is soluble in hot strong acid and hot strong alkali, but insoluble in ethanol and water. As a new type of n-type semiconductor metal oxide, its conductivity and visible light transmittance are very high, and its bandgap width is mainly between 3.55-3.75 eV. 2 O 3 The specific surface area and surface activity of indium oxide are large, so indium oxide gas-sensitive materials have excellent properties in light, electricity, chemistry, etc., and can be widely used in solar cells, gas sensors, optoelectronic devices, flat panel displays, diodes and other fields. After years of research, it was found that In 2 O 3 Gas sensors can be used to detect gases such as isopropyl alcohol, ethanol, nitrogen dioxide, and hydrogen.
[0003] In 2 O 3 The preparation technology has made remarkable progress, especially In 2 O 3 It has begun to be applied to the field of gas sensor design. At present, the research on its preparation technology is increasing. Many researchers have designed different preparation methods. The most commonly used methods are chemical coprecipitation, water solvent thermal method, organic solution synthesis method, hot injection method, sol-gel method, microemulsion method, thermal evaporation oxidation method, arc discharge method, etc. The principles of various methods are different, and the morphologies of the prepared indium oxide are also different. In the currently published literature, the hydrothermal method for preparing nano indium oxide is the most common. Researchers have prepared indium oxide with different morphologies, such as nanoparticles, nanofilms, nanobelts, and nanowires / rods, by regulating different reaction conditions and additives. However, the existing methods for preparing nano indium oxide usually have the following disadvantages: 1) The reaction conditions are harsh, the cost is too high, and it is difficult to produce on a large scale; 2) The obtained indium oxide products are easy to agglomerate; 3) The reaction temperature requirements are high, the control is difficult, and the operation is inconvenient; 4) The prepared indium oxide has a relatively low gas-sensitive performance to gas, which reduces the use effect of indium oxide nanomaterials. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides an indium oxide nanomaterial with a composite morphology, which is improved and optimized on the basis of the ordinary hydrothermal method. By strictly adjusting the ratio and dosage of urea, indium nitrate and sodium dodecyl sulfate, and adopting microwave treatment, an indium oxide nanomaterial with a specific morphology is formulated, and the material has an excellent detection effect on VOC gases.
[0005] The present invention adopts the following technical solutions:
[0006] A composite indium oxide nanomaterial is prepared by the following method:
[0007] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0008] (2) placing solution A in a stirring device and continuously stirring it, adding a certain amount of sodium dodecyl sulfate thereto, and continuing stirring for 10 minutes to obtain solution B;
[0009] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 min to obtain solution C;
[0010] (4) Rapidly add solution C to solution B while stirring, and continue stirring for a period of time to obtain solution D;
[0011] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep it warm for a period of time, and then cool it to obtain the product;
[0012] (6) The product obtained in step (5) is first subjected to multiple centrifugal washings with water and then multiple alcohol washings, and then dried to obtain a solid product;
[0013] (7) The solid product obtained in step (6) is placed in a microwave oven for microwave heating for 1 min, and then cooled to room temperature to obtain the indium oxide nanomaterial with a clustered morphology as described in the present invention.
[0014] Preferably, the molar ratio of indium nitrate to urea is 1:1.5-2; the concentration of solution A is 0.06 g / mL; and the concentration of solution C is 0.045-0.06 g / mL.
[0015] Preferably, the mass ratio of the sodium dodecyl sulfate to indium nitrate is 1:300.
[0016] Preferably, the continuous stirring reaction time in step (4) is 20 minutes.
[0017] Preferably, the insulation reaction time in step (5) is 10 minutes.
[0018] Preferably, in step (6), the drying temperature is 65° C. and the drying time is 8 hours.
[0019] Preferably, the microwave heating power in step (7) is 900W.
[0020] The indium oxide nanomaterial prepared by the present invention is a highly dispersed cluster structure, which is composed of a cubic and a sheet structure. The structure has a high specific surface area, increases the gas adsorption sites, and significantly improves the gas-sensing performance of the material, especially has excellent sensitivity to VOC gas.
[0021] The present invention also provides an application of a composite-morphology indium oxide nanomaterial in VOC gas detection. The indium oxide nanomaterial prepared by the present invention has good sensitivity and selectivity to common VOC gases such as formaldehyde, acetone, toluene, ethanol, and ethylene glycol due to its special structure.
[0022] In the present invention, urea is used as an alkali source, and OH is slowly released through hydrolysis. - , and with In 3+ The reaction generates In(OH) 3 ,In(OH) 3 Heating decomposition generates In 2 O 3 By controlling the carbon source and In 3+ The molar ratio of 1:1 was used to strictly control the hydrolysis reaction rate, and the surfactant sodium dodecyl sulfate SDS was added as a directing agent. The microwave heating method was used as a crystal surface growth blocking and regulation method to make a large amount of In(OH) 3 The crystals do not have enough time to deposit along a specific crystal plane, so the indium oxide nanomaterial with a specific composite morphology of the present invention is formed. The surfactant SDS, urea, and microwave heating play a synergistic role in the formation of the morphology, and the composite morphology cannot be obtained without any one of them.
[0023] The beneficial effects of the present invention are as follows: the present invention prepares a nano-indium oxide with a highly dispersed cluster structure, which is conducive to the sparse diffusion of gas and has excellent sensitivity to VOC gas, wherein the detection limit of formaldehyde can reach 5ppm; the nano-indium oxide is prepared by a microwave heating method, which heats quickly, saves energy, reduces energy consumption and reduces emissions, promotes green development, and is conducive to industrial production; ordinary hydrothermal treatment takes several hours to dozens of hours, while this method only takes a few minutes, and the efficiency is widely improved; In(OH) 3 The microwave method is used to heat and decompose into indium oxide, the time is short, the crystal generation speed is fast, the Ostwald ripening time is short, and the agglomeration phenomenon caused by sintering in the traditional hydrothermal method using a muffle furnace heating process can be effectively prevented, thereby preparing the nano indium oxide product with a highly dispersed cluster structure of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 In prepared in Example 2 of the present invention 2 O 3 X-ray diffraction pattern of
[0025] Figure 2 In prepared in Example 2 of the present invention 2 O 3 TEM images of
[0026] Figure 3 In prepared in Example 2 of the present invention 2 O 3 Sensitivity data graph to different concentrations of formaldehyde at room temperature;
[0027] Figure 4 In prepared in Example 2 of the present invention 2 O 3 Detection response diagram of various VOC gases. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with specific embodiments and drawings. Example 1
[0029] A composite indium oxide nanomaterial is prepared by the following method:
[0030] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0031] (2) Place solution A in a stirring device and stir it continuously, add SDS thereto, and continue stirring for 10 minutes to obtain solution B; the mass ratio of SDS to indium nitrate is 1:300;
[0032] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 minutes to obtain solution C; the molar ratio of indium nitrate to urea is 1:1.5; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.045 g / mL;
[0033] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0034] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0035] (6) The product obtained in step (5) was first centrifuged and washed with water for multiple times, then washed with alcohol for multiple times, and dried at 65° C. for 8 h to obtain a solid product;
[0036] (7) The solid product obtained in step (6) was placed in a microwave oven and the microwave power was set to 900 W. After microwave heating for 1 min, the solid product was cooled to room temperature to obtain the indium oxide nanomaterial with cluster morphology as described in the present invention. Example 2
[0037] A composite indium oxide nanomaterial is prepared by the following method:
[0038] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0039] (2) Place solution A in a stirring device and stir it continuously, add SDS thereto, and continue stirring for 10 minutes to obtain solution B; the mass ratio of SDS to indium nitrate is 1:300;
[0040] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 min to obtain solution C; the molar ratio of indium nitrate to urea is 1:1.8; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.05 g / mL.
[0041] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0042] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0043] (6) The product obtained in step (5) was first centrifuged and washed with water for multiple times, then washed with alcohol for multiple times, and dried at 65° C. for 8 h to obtain a solid product;
[0044] (7) The solid product obtained in step (6) was placed in a microwave oven and the microwave power was set to 900 W. After microwave heating for 1 min, the solid product was cooled to room temperature to obtain the indium oxide nanomaterial with cluster morphology as described in the present invention. Example 3
[0045] A composite indium oxide nanomaterial is prepared by the following method:
[0046] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0047] (2) Place solution A in a stirring device and stir it continuously, add SDS thereto, and continue stirring for 10 minutes to obtain solution B; the mass ratio of SDS to indium nitrate is 1:300;
[0048] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 min to obtain solution C; the molar ratio of indium nitrate to urea is 1:2; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.06 g / mL.
[0049] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0050] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0051] (6) The product obtained in step (5) was first centrifuged and washed with water for multiple times, then washed with alcohol for multiple times, and dried at 65° C. for 8 h to obtain a solid product;
[0052] (7) The solid product obtained in step (6) was placed in a microwave oven and the microwave power was set to 900 W. After microwave heating for 1 min, the solid product was cooled to room temperature to obtain the indium oxide nanomaterial with cluster morphology as described in the present invention.
[0053] Comparative Example 1
[0054] A composite indium oxide nanomaterial is prepared by the following method:
[0055] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0056] (2) Place solution A in a stirring device and stir it continuously, add SDS thereto, and continue stirring for 10 minutes to obtain solution B; the mass ratio of SDS to indium nitrate is 1:300;
[0057] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 minutes to obtain solution C; the molar ratio of indium nitrate to urea is 1:1.5; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.045 g / mL;
[0058] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0059] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0060] (6) The product obtained in step (5) was first subjected to multiple centrifugal washings with water and then multiple alcohol washings, and then dried at 65°C for 8 h to obtain the final target product.
[0061] This comparative example is basically the same as Example 1, except that there is no microwave heating treatment step (7).
[0062] The obtained nano indium oxide powder does not have the highly dispersed cluster structure of the present invention.
[0063] Comparative Example 2
[0064] A composite indium oxide nanomaterial is prepared by the following method:
[0065] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0066] (2) Place solution A in a stirring device and stir continuously for 10 min to obtain solution B;
[0067] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 minutes to obtain solution C; the molar ratio of indium nitrate to urea is 1:1.5; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.045 g / mL;
[0068] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0069] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0070] (6) The product obtained in step (5) was first centrifuged and washed with water for multiple times, then washed with alcohol for multiple times, and dried at 65° C. for 8 h to obtain a solid product;
[0071] (7) The solid product obtained in step (6) was placed in a microwave oven and the microwave power was set to 900 W. After microwave heating for 1 min, the solid product was cooled to room temperature to obtain an indium oxide nanomaterial.
[0072] This comparative example is basically the same as Example 1, except that SDS is not added in step (2).
[0073] The obtained nano indium oxide powder does not have the highly dispersed cluster structure of the present invention.
[0074] Comparative Example 3
[0075] A composite indium oxide nanomaterial is prepared by the following method:
[0076] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0077] (2) Place solution A in a stirring device and stir it continuously, add SDS thereto, and continue stirring for 10 minutes to obtain solution B; the mass ratio of SDS to indium nitrate is 1:300;
[0078] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 min to obtain solution C; the molar ratio of indium nitrate to urea is 1:3; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.045 g / mL;
[0079] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0080] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0081] (6) The product obtained in step (5) was first centrifuged and washed with water for multiple times, then washed with alcohol for multiple times, and dried at 65° C. for 8 h to obtain a solid product;
[0082] (7) The solid product obtained in step (6) was placed in a microwave oven and the microwave power was set to 900 W. After microwave heating for 1 min, the solid product was cooled to room temperature to obtain an indium oxide nanomaterial.
[0083] This comparative example is basically the same as Example 1, except that the molar ratio of indium nitrate to urea in step (3) is different.
[0084] The obtained nano indium oxide powder does not have the highly dispersed cluster structure of the present invention.
[0085] Comparative Example 4
[0086] A composite indium oxide nanomaterial is prepared by the following method:
[0087] (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A;
[0088] (2) Place solution A in a stirring device and stir it continuously, add SDS thereto, and continue stirring for 10 minutes to obtain solution B; the mass ratio of SDS to indium nitrate is 1:300;
[0089] (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 min to obtain solution C; the molar ratio of indium nitrate to urea is 1:4; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.045 g / mL;
[0090] (4) Rapidly add solution C to solution B while stirring, and continue stirring for 20 min to obtain solution D;
[0091] (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep the temperature for 10 minutes, and cool to obtain the product;
[0092] (6) The product obtained in step (5) was first centrifuged and washed with water for multiple times, then washed with alcohol for multiple times, and dried at 65° C. for 8 h to obtain a solid product;
[0093] (7) The solid product obtained in step (6) was placed in a microwave oven and the microwave power was set to 900 W. After microwave heating for 1 min, the solid product was cooled to room temperature to obtain an indium oxide nanomaterial.
[0094] This comparative example is basically the same as Example 1, except that the molar ratio of indium nitrate to urea in step (3) is different.
[0095] The obtained nano indium oxide powder does not have the highly dispersed cluster structure of the present invention.
[0096] In order to better illustrate the effect of the present invention, the product prepared in Example 2 was further tested. First, the product of Example 2 was subjected to an X-ray diffraction test. The specific results are as follows: Figure 1 shown. Figure 1 The median is 21.8, 30.8, 35.7, 38.1, 42.1, 45.9, 51.3, 56.3, 59.4, 60.8, 62.4 and 63.9 o The diffraction peaks at correspond to In 2 O 3 The (211), (222), (400), (411), (332), (431), (440), (611), (541), (622), (631) and (444) crystal planes. The (222) diffraction peak is relatively stronger and sharper, which indicates that the crystal grows preferentially along the
[111] direction. All diffraction peaks are consistent with the cubic phase In 2 O 3 The standard spectrum of (JCPDS No. 06-0416) is completely consistent. No other impurity peaks were detected, which shows that high-purity In 2 O 3 Cubic phase crystal system, the product has good crystallization performance. In order to further obtain the size and morphology characteristics of the product of the present invention, the product of Example 2 was tested by scanning electron microscopy. Figure 2 Field emission scanning electron microscope images at different magnifications. Figure 2It can be seen from ac that the product of the present invention is a highly dispersed cluster structure with a cluster diameter of 3-4 μm. The cluster structure is composed of a combination of cubic and lamellar structures. The structure has a high specific surface area, increases the gas adsorption sites, and significantly improves the gas-sensitive performance of the material.
[0097] In order to better illustrate the gas-sensing performance of the product of the present invention, the product of the present invention is used to detect formaldehyde gas, and the test data show that ( Figure 3 The composite nano-indium oxide prepared by the method of the present invention shows good gas sensing performance and can still detect 5ppm. The composite nano-indium oxide material prepared by the present invention has good selectivity for common VOC gases such as formaldehyde, acetone, and toluene. The test data are as follows: Figure 4 shown.
[0098] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a composite morphology indium oxide nanomaterial, characterized in that: The preparation method comprises the following steps: (1) Accurately weigh indium nitrate and dissolve it in deionized water to obtain solution A; (2) Place solution A in a stirring device and stir it continuously, add a certain amount of sodium dodecyl sulfate into solution A, and continue stirring for 10 minutes to obtain solution B; (3) Accurately weigh urea, add it into deionized water under stirring until it is completely dissolved and continue stirring for 15 min to obtain solution C; (4) Rapidly add solution C to solution B while stirring, and continue stirring for a period of time to obtain solution D; (5) Add solution D into the microwave hydrothermal reaction quartz tube, adjust the heating rate so that the temperature rises to 120°C within 1 minute, keep it warm for a period of time, and then cool it to obtain the product; (6) The product obtained in step (5) is first subjected to multiple centrifugal washings with water and then multiple alcohol washings, and then dried to obtain a solid product; (7) placing the solid product obtained in step (6) in a microwave oven for microwave heating for 1 min, and then cooling to room temperature to obtain an indium oxide nanomaterial with a clustered morphology; The molar ratio of indium nitrate to urea is 1:1.5-2; the concentration of solution A is 0.06 g / mL; the concentration of solution C is 0.045-0.06 g / mL; The mass ratio of sodium dodecyl sulfate to indium nitrate is 1:300; The continuous stirring reaction time in step (4) is 20 minutes; The heat preservation reaction time in step (5) is 10 minutes; In step (6), the drying temperature is 65° C. and the drying time is 8 h; The microwave heating power in step (7) is 900W.
Citation Information
Patent Citations
Method for preparing nano indium oxide with controllable appearance by hydrothermal method
CN101857263A
Method for preparing indium oxide cubes through microwave-assisted hydrothermal method
CN103408064A
Triple-mesopore indium oxide formaldehyde gas-sensitive material and preparation method thereof
CN104495912A
Preparation method of hierarchical-structured indium oxide microsphere composed of cubes
CN106186048A
Appearance-controllable indium oxide powder and low-temperature hydrothermal synthesis method thereof
CN107140682A
Cited By
Preparation method and application of indium oxide catalyst
CN120037894A