A method for preparing assembled ancient building wall
Through the structural optimization of the facing brick layer and the use of improved epoxy interface agents, the stability problem of the connection between the brick layer and the concrete layer in the prefabricated antique buildings has been solved, and the bonding force, water resistance, and alkali resistance have been improved. safety, simplifying the construction process and reducing costs.
Patent Information
- Application Number
- CN202410388766.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-01
Smart Images

Figure CN118181503B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a novel building industrialized wall, in particular to a preparation method of an assembled ancient building wall. Background Art
[0002] Traditional ancient building wall construction generally has problems such as cumbersome procedures, high pollution, serious material consumption, and uncontrollable energy-saving coefficient. In order to develop a greener, energy-saving, and efficient ancient building construction system, we specially carry out prefabricated research and development and application for the walls in ancient buildings. Prefabricated buildings refer to buildings assembled on site with prefabricated components. For example, the building walls have been prefabricated in the factory. When building on the site, you only need to install the prefabricated walls to the designated location and then cast them into shape. Prefabricated buildings are easy to install, have a short construction period, and have stable building structure quality, and can form an industrialized production and processing system.
[0003] At present, the common prefabricated sandwich insulation system is composed of two layers of inner and outer reinforced concrete wall panels and the insulation material sandwiched therebetween through special connectors. The outer wall panels have specific insulation performance requirements and provide effective protection for the inner wall panels and the insulation material. Reinforcements are provided between the inner and outer panels, which are connected through existing special connectors. For example, CN114135048A discloses a sandwich insulation composite shear wall and connectors, including: a prefabricated outer panel layer, an insulation panel layer, a cavity layer, a prefabricated inner panel layer, and connectors for connecting the prefabricated outer panel layer, the insulation panel layer, the cavity layer, and the prefabricated inner panel layer; wherein the connectors include: a concave head screw section, a threaded sleeve section, and a first tail section.
[0004] At present, in addition to the restoration of cultural relics, antique buildings generally use modern materials and imitate ancient styles. Prefabricated buildings are increasingly used in the construction of antique buildings due to their energy-saving and environmental protection advantages. The biggest difference between traditional Chinese ancient buildings and traditional Western buildings is the wooden structure system. Traditional buildings are not simply made of wood. A large number of bricks and stones are used in traditional buildings, including walls, tiles, floors, etc., which are all made of bricks. Therefore, the exterior wall decoration of ancient Chinese buildings is usually represented by brickwork.
[0005] At present, the technical difficulty of combining modern prefabricated buildings with Chinese antique buildings lies in the combination of external decorative brickwork layers and internal concrete layers. The main structure of the existing prefabricated building wall is concrete, and there is generally no decorative brickwork layer. Even if there is, generally speaking, brickwork is laid first, and then concrete prefabricated walls are used. In the existing prefabricated antique building insulation wall structure, the walls are generally connected to each other by bolts and other connectors. The decorative brickwork layer and concrete layer of the current prefabricated ancient building are also connected by connectors. For example, CN115584805 discloses an assembled antique building insulation wall structure, including a connecting component and a wall component, the connecting component includes a connecting block, a slot, a connecting groove, a limit block, a sliding rod, a spring and an insert block; the upper surface and the lower surface of the connecting block are symmetrically provided with two slots, and the top and the bottom of the connecting groove are symmetrically slidably connected with two sliding rods; the wall component includes a connecting rod, a first blue brick, a second blue brick and a positioning groove. The problem with the above-mentioned prefabricated technology is that it still uses a complex connection mechanism to connect the brick wall composed of blue bricks and the concrete insulation wall. The construction process is complicated and the efficiency is low. It has high requirements for construction personnel and the manufacturing cost has remained high. In addition, the existence of the connecting parts has an impact on the paving of the facing bricks, especially the facing brick layer with an external configuration, and will also affect the overall strength of the facing brick layer.
[0006] It can be seen that the outer brickwork layer and the inner insulation wall of the current prefabricated antique building insulation wall structure are actually prefabricated separately, and are fixed and connected by connectors during installation. Therefore, the market needs prefabricated antique buildings that can be formed in one piece in the factory in advance, which reduces the number of connectors and the quality risks of the connections between different walls. Although some documents currently disclose the use of interface agents to bond polymer decorative layers, or polymer thermal insulation layers and inorganic layers, for example, common acrylic interface agents and epoxy acrylic interface agents have good bonding properties for polymer material layers and inorganic material layers, CN104650302A discloses an interface agent, which is prepared from the following components in mass percentage: 5-8.5% n-butyl acrylate, 3-10.2% methyl methacrylate, 0-1.2% acrylic acid, 0-0.2% initiator, 0.2-1.5% composite emulsifier, 0-8% epoxy resin, 61-78% water, 4-8.2% styrene, 0.3-1.5% propylene glycol, and 0-0.3% sodium bicarbonate. The interface agent has the advantages of excellent construction performance, good interface tensile bonding strength, superior aging resistance, long storage period, etc. When applied to interface areas such as building insulation composite external formwork and insulation decorative panels, it can overcome the defects of low bonding strength between traditional interface agents and insulation materials and mortar, and easy hollowing and cracking of insulation materials. However, the inventors found that the bonding force between the face brick layer and the slow-setting soil layer of the current interface agent cannot meet the requirements of engineering construction, especially during the hoisting process, the face brick layer has a gravity several dozen or even hundreds of times higher than that of the polymer decorative layer and insulation layer in the above-mentioned literature, and has particularly high requirements for bonding performance. In addition, the complex inorganic material system on the front and back surfaces puts forward higher requirements on the corrosion resistance, water resistance, and alkali resistance of the interface agent.
[0007] Therefore, the main technical problem that needs to be solved in the thermal insulation wall structure of prefabricated antique buildings is how to achieve a safe, long-term and stable connection between the outer brick layer and the inner thermal insulation concrete wall. Summary of the invention
[0008] The invention discloses a method for preparing an assembled ancient building wall, wherein the assembled ancient building wall is 210-330 mm thick, preferably 250-300 mm thick, and comprises, from the outer wall to the inner wall, a 30-50 mm thick face brick layer, a 40-60 mm thick outer concrete page layer, a 60-100 mm thick insulation layer, and an 80-120 mm thick inner concrete structure wall layer, and the preparation method comprises the following steps:
[0009] 1) Mold cleaning;
[0010] 2) Arrange the bricks and fill the seams with sponge strips to obtain the facing brick layer, and make grooves on the side of the facing brick layer close to the outer page layer;
[0011] 3) Cement mortar filling;
[0012] 4) Apply interface agent by brush;
[0013] 5) Lay the first layer of steel bars and set the upper and lower layer steel bar tie embedded parts;
[0014] 6) pouring concrete to obtain the outer layer;
[0015] 7) Laying the insulation layer;
[0016] 8) Lay the second layer of steel bars, connect the first and second layers of steel bars, and pre-embed water and electricity pipelines, hoisting parts, and connectors;
[0017] 9) pouring the inner layer of concrete;
[0018] 10) Wall demoulding, maintenance and acceptance.
[0019] The wall is a sill wall, a gable wall or a rear eaves wall.
[0020] Among them, the concrete in the inner layer of the concrete structure wall is preferably lightweight aggregate concrete.
[0021] The heat-insulating material of the heat-insulating layer is a molded polystyrene board, an extruded polystyrene board or a foamed polystyrene board.
[0022] The sill wall is dry-laid, and the sill wall core is made of Begonia pond hard core square bricks. The dry-laid wall surface brick arrangement should be tested in advance, and the front test of each brick joint is confirmed to be correct before it can be reversed in the mold.
[0023] The gable is a moon-white soft-core wall; the soft-core wall needs to reserve plastering thickness, otherwise the plastering thickness of the mortar joints at the joints of the wall panels during the later wall treatment will not reach the plastering layer and will easily fall off.
[0024] The rear eaves wall is painted with small mud and whitewashing method.
[0025] Among them, wooden space is reserved in the window area, and vertical bricks are used under the window.
[0026] In order to avoid the formation of through-joint seams at the junction of wall panels, a tooth-shaped joint area is reserved for subsequent masonry construction (the same applies to wall corners).
[0027] The facing bricks used are from the same batch of bricks fired in the same furnace to ensure a uniform overall wall effect and reduce color differences.
[0028] The corner flowers and line squares in the core of the sill wall square bricks are made by the factory with unified molds and unified specifications for production and processing control, which reduces the uncertainty of errors that may occur during manual on-site polishing, speeds up the wall panel production cycle, and further improves the wall panel production efficiency.
[0029] In the mold cleaning step, the mold is first inspected and accepted, and the corresponding wall mold is carefully checked and accepted according to the dimensions specified in the design drawings, and the overall dimensions of the mold, the staggered dimensions, the firmness of the connecting parts, and the flatness and smoothness of the bottom plate are checked and checked.
[0030] Since each wall panel is heavy, a crane is required for lifting. Therefore, corresponding lifting parts and connecting parts required for connecting and fixing various parts of the wall panel need to be embedded in the wall panel. The embedded lifting parts should be firmly connected to the structural steel bars of the wall panel and sealed inside the wall panel.
[0031] During the research process, the inventors found that the key technology to obtain a prefabricated wall in which the brick layer (i.e., the face brick layer) and the thermal insulation concrete wall are integrally formed is the connection problem between the brick layer and the thermal insulation concrete wall. Compared with the currently used connectors, when integrally formed, improving the interlayer adhesion between the face brick layer and the concrete wall is the first technical problem to be solved, so as to avoid cracking between different layers during movement, and also prevent cracks between the face brick layer and the concrete wall over time. The inventors have tried a large number of existing adhesives to improve the adhesion between the face brick layer and the concrete wall layer, but they are either prone to cracking during hoisting, or are not water-resistant and alkali-resistant. Over time, the bonding performance of the adhesive decreases, and cracks will gradually appear, which makes the prefabricated ancient building wall have quality risks. The inventors and the interface agent supplier conducted joint scientific research on the structure of the wall and the type of adhesive, and found that the following process can significantly improve the interlayer adhesion between the face brick layer and the concrete wall, and it is effective for a long time:
[0032] (1) The structure of the brick layer is optimized by grooving to increase the wall bonding pull-out force and ensure the stability and safety of the brick layer, wherein the cross-sectional shape of the groove is square, rectangular or trapezoidal, and more preferably trapezoidal.
[0033] (2) Applying an epoxy interface agent having strong bonding properties, alkali resistance and water resistance on the side of the face brick layer facing the outer layer of concrete, wherein the interface agent is prepared by mixing component A and component B in a weight ratio of (4-6):1.
[0034] Component A comprises the following components by weight: 60-80 parts of epoxy acrylic resin, 10-20 parts of active diluent, 5-10 parts of auxiliary agent, 10-30 parts of conventional diluent A, and 20-30 parts of filler.
[0035] Component B contains: 10-30 parts of curing agent and conventional diluent B.
[0036] The auxiliary agents include wetting agents, leveling agents, defoaming agents, dispersants and anti-settling agents.
[0037] Further, the wetting agent is H-140;
[0038] The defoamers were Evonik Chemicals AIREX 900 and BYK-1794;
[0039] The leveling agent is BYK 354;
[0040] The dispersants are BYK 110 and BYK 163 from BYK Chemical;
[0041] The anti-settling agent is fumed silica, selected from R972 and R816 of Degussa.
[0042] The filler includes silicon micropowder, titanium dioxide, calcite powder, heavy calcium carbonate and talcum powder.
[0043] The preparation method of the interface agent comprises the following steps:
[0044] (1) mixing and stirring the epoxy acrylic resin, reactive diluent, auxiliary agent, and conventional diluent A in a high-speed disperser to obtain a mixture;
[0045] (2) adding filler to the mixture obtained in step (1) in a disperser while stirring to obtain component A;
[0046] (3) The curing agent and conventional diluent B are mixed and stirred using a disperser to prepare component B.
[0047] In step (1), the rotation speed of the high-speed disperser is 800-1000 rpm, and the stirring time is 15-20 min.
[0048] In step (2), the rotation speed of the disperser is 1200-1500 rpm, and the stirring time is 30-45 min.
[0049] In step (3), the rotation speed of the disperser is 600-800 rpm, and the stirring time is 5-10 min.
[0050] The epoxy acrylic resin is prepared by free radical copolymerization of a first monomer, a second monomer and a third monomer.
[0051] The first monomer is an acrylate monomer having three or more unsaturated carbon-carbon double bonds, and specifically may be trimethylolpropane trimethacrylate.
[0052] The second monomer is a monomer having an unsaturated carbon-carbon double bond and an epoxy group, and specifically can be glycidyl methacrylate.
[0053] The third monomer is γ-methacryloxypropyltrimethoxysilane.
[0054] The mass ratio of the first monomer, the second monomer and the third monomer is 2:(4-6):(0.4-0.6), and the preferred mass ratio is 2:5:0.5. The amount of the first monomer cannot be too much compared to the second monomer with unsaturated carbon-carbon double bonds and epoxy groups. If it is too much, the cross-linking density is too high. Although the adhesion is good, the flexibility of the interface layer is poor, and it is easy to crack when encountering instantaneous rigid force. If the amount is too little, it is not easy to obtain strong adhesion. As for the amount of the third monomer, if the amount is too much, the cost is too high, and if the amount is too little, the effect of improving the adhesion, water resistance and alkali resistance of the interface agent is not obvious.
[0055] The preparation method of epoxy acrylic resin comprises dissolving the first monomer, the second monomer and the third monomer in an organic solvent system under stirring, heating after they are completely dissolved, adding an initiator, and reacting for 3-5 hours in a reflux manner to obtain an epoxy acrylic resin solution, wherein the resin has an organosilicon functional group.
[0056] Amine curing agent: selected from triethylenetetramine, polyamide or polyetheramine and / or aminopropyltriethoxysilane (KH550), preferably a mixture of polyamide (POLYPOXW804, aradur-450, Versamid 228) and γ-aminopropyltriethoxysilane KH550, wherein the mass ratio of polyamide to γ-aminopropyltriethoxysilane is (8-10):1.
[0057] The active diluent is 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, fatty glycidyl ether and / or butyl glycidyl ether, preferably a combination of active diluents with a mass ratio of 1,4-butanediol diglycidyl ether and butyl glycidyl ether of (1-2):1. This is because 1,4-butanediol diglycidyl ether not only has two epoxy groups, but also has a longer chain, and cross-links to form chains and networks during curing, which can significantly improve the tensile strength, impact strength and other properties of the interface layer. Butyl glycidyl ether contains both ether bonds and epoxy groups in the molecule, which not only has an excellent dilution effect, but also produces hydrogen bonds between the ether bonds, which can also give the interface layer a strong adsorption force. Therefore, 1,4-butanediol diglycidyl ether and butyl glycidyl ether as active diluents can significantly improve the mechanical properties of the interface layer while ensuring good adhesion, and the ability to reduce viscosity and dilution is very excellent.
[0058] Conventional diluent A may be xylene, butyl acetate, propylene glycol methyl ether acetate, ethylene glycol methyl ether, ethylene glycol butyl ether, acetone, butanone and or cyclohexanone.
[0059] Conventional diluent B may be xylene, butyl acetate, propylene glycol methyl ether acetate, butanol, butanone and cyclohexanone and or isopropanol.
[0060] Furthermore, after applying the epoxy interface agent, a layer of inorganic interface agent can be applied to further improve the affinity with the concrete wall layer, thereby improving the adhesion performance.
[0061] After adopting the above technical solution, the present invention has at least the following beneficial effects:
[0062] (1) After extensive research, the inventors found that by optimizing the structure of the tile layer, that is, by using a groove treatment method, not only the construction area of the interface agent is increased, the wall bonding pull-out force is increased, and the stability and safety of the tile layer are ensured. At the same time, the special-shaped connection between the tile layer and the concrete layer produces a snap-fit effect. The vertical snap-fit and the interface bonding force of the groove three surfaces are significantly improved compared to the common single-sided bonding.
[0063] Furthermore, the cross-sectional shape of the groove is square, rectangular or trapezoidal, more preferably trapezoidal. This is because after the concrete solidifies, the trapezoidal snap-fit connection between the facing brick layer and the concrete layer has not only vertical snap-fitting, but also horizontal snap-fitting. Combined with the bonding force of the interface agent, the interlayer bonding force between the facing brick layer and the concrete layer is further greatly enhanced.
[0064] (2) During the research and development of the prefabricated ancient building wall, the inventors worked with the interface agent supplier to improve the original interface agent based on the product characteristics. Although the cost has increased, the adhesion, water resistance and alkali resistance have been significantly improved. First, the main epoxy resin is a silicone-modified acrylic epoxy resin obtained by polymerizing an acrylate monomer with more than three unsaturated carbon-carbon double bonds, a monomer with unsaturated carbon-carbon double bonds and epoxy groups, and an unsaturated silicone such as γ-methacryloxypropyltrimethoxysilane. The epoxy resin has the characteristics of excellent adhesion, water resistance and good alkali resistance, and the acrylate with more than three unsaturated carbon-carbon double bonds produces a network cross-linked interpenetrating system with it, which greatly improves the density of the epoxy group, making the modified epoxy resin adhesion, water resistance and alkali resistance significantly improved compared with general epoxy resins, and the polyacrylate in the modified epoxy resin brings its inherent flexibility, which can effectively improve the tensile strength and other mechanical properties of the interface layer, and prevent the interface layer from lacking toughness due to excessive cross-linking density. The addition of unsaturated silicone monomers makes the modified epoxy resin contain polysilane, which not only brings hydrophobicity to the epoxy resin, but also the presence of a large number of hydroxyl groups improves the adhesion of the interface agent and further enhances the water and alkali resistance of the interface agent.
[0065] In addition, the interface agent in this application also uses an active diluent, which reduces the use of solvents, increases the curing speed of the interface agent at room temperature or even in winter, and reduces the negative impact of excessive solvent use on the solidification and maintenance of adjacent concrete layers, allowing the next concrete pouring process to be implemented within 30-60 minutes, greatly improving production efficiency.
[0066] The curing agent of the interface agent is preferably polyamide and γ-aminopropyl triethoxysilane. The polyamide curing agent has an internal plasticizing effect, which greatly improves the toughness of the interface agent layer. It also has amide groups and hydroxyl groups. The cured epoxy resin system has excellent adhesion, and has a polar amino group at one end and a non-polar long-chain hydrocarbon group at the other end. Therefore, it can adhere to and replace the water film on the wet surface. Therefore, the interface agent made by the polyamide curing agent has good adhesion to the concrete layer formed by the subsequent concrete pouring process, and there is no need to worry about the negative impact of the water-containing concrete on the interface agent. When γ-aminopropyl triethoxysilane is added to the curing agent, its amino group not only cross-links and cures with the epoxy resin to increase the cross-linking density, but also introduces the hydrophobicity of organic silicon to improve water resistance and alkali resistance. At the same time, the silanol generated by its hydrolysis, together with the silanol in the modified epoxy resin, can produce a strong coupling anchoring effect with the inorganic material of the concrete layer, significantly improving the bonding force of the interface agent.
[0067] (3) The prefabricated wall panels are processed in an integrated factory and then transported to the site for hoisting, which avoids wet work on site, effectively solves the construction restrictions of ancient buildings in winter, and provides assistance to speed up the project construction progress;
[0068] (4) Factory-based room temperature production conditions and maintenance effectively guarantee the quality of ancient building prefabricated wall panels. At the same time, ancient building prefabricated wall panels basically eliminate the inevitable alkali reaction phenomenon during winter construction, achieving better quality results.
[0069] (5) Small lifting machines such as spider cranes solve the problem of lifting operations in narrow spaces;
[0070] (6) The 5mm sponge strip used for mortar joint control effectively controls the mortar joints on the wall during wall panel processing, and is easy to clean without affecting subsequent construction. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] Figure 1 A schematic diagram of the structure of the present invention
[0072] In the accompanying drawings: 1, facing brick layer, 2, outer page layer, 3, insulation layer, 4, inner page layer. DETAILED DESCRIPTION
[0073] The technical solution of the invention is described in detail below in conjunction with specific embodiments.
[0074] Example 1 Preparation of epoxy type interface agent
[0075] The interface agent is prepared by mixing component A and component B in a weight ratio of 6:1;
[0076] Component A comprises the following components in parts by weight: 60 parts of epoxy acrylic resin, 15 parts of active diluent, 5 parts of auxiliary agent, 20 parts of conventional diluent A, and 20 parts of filler.
[0077] The active diluent is a combination of 1,4-butanediol diglycidyl ether and butyl glycidyl ether in a mass ratio of 1:1, each of which is 7.5 parts. The auxiliary agents are 1 part of wetting agent, 0.5 part of leveling agent, 1 part of defoaming agent, 2 parts of dispersant, and 0.5 part of fumed silica anti-settling agent.
[0078] The filler includes 7.5 parts of silicon micropowder, 7.5 parts of talc powder and 5 parts of titanium dioxide.
[0079] Component B comprises: 15 parts of a curing agent, 5 parts of a conventional diluent B, and a mixture of polyamide and γ-aminopropyltriethoxysilane in a mass ratio of 9:1.
[0080] Conventional diluent A and conventional diluent B are both propylene glycol methyl ether acetate.
[0081] The epoxy acrylic resin is prepared by free radical copolymerization of trimethylolpropane trimethacrylate, glycidyl methacrylate and γ-methacryloxypropyl trimethoxysilane in a mass ratio of 2:5:0.5. The specific preparation method comprises dissolving the three monomers in an organic solvent system under stirring, heating after they are completely dissolved, adding an initiator, and reacting for 4 hours in a reflux manner to obtain an epoxy acrylic resin solution.
[0082] The preparation method of the interface agent comprises the following steps:
[0083] (1) mixing and stirring the epoxy acrylic resin, reactive diluent, auxiliary agent, and conventional diluent A in a high-speed disperser to obtain a mixture;
[0084] (2) adding filler to the mixture obtained in step (1) while stirring to obtain component A;
[0085] (3) The curing agent and conventional diluent B are mixed and stirred using a disperser to obtain component B. When in use, component A and component B are blended again.
[0086] In step (1), the rotation speed of the disperser is 800 rpm, and the stirring time is 20 min.
[0087] In step (2), the rotation speed of the disperser is 1200 rpm, and the stirring time is 40 min.
[0088] The speed of the disperser in step (3) is 600 rpm, and the stirring time is 8 min.
[0089] Example 2 Preparation of assembled ancient building threshold wall A
[0090] The thickness of the assembled ancient building threshold wall is 270 mm, specifically including a 40 mm thick face brick layer 1, a 50 mm thick outer page layer 2, an 80 mm thick insulation layer 3 and a 100 mm thick inner page layer 4. For example, the face brick layer 1 can be a small mud face brick layer, the outer page layer 2 can be a concrete outer page layer, the insulation layer 3 can be an extruded polystyrene board insulation layer, and the inner page layer 4 can be a lightweight aggregate concrete structure wall inner page layer, which includes the following steps:
[0091] 1) Mold cleaning;
[0092] 2) Arranging bricks and plugging seams with sponge strips to obtain a facing brick layer, and performing groove processing on the facing brick layer, wherein the cross-sectional shape of the groove is a trapezoidal structure, which is a type that is wide at the bottom and narrow at the top;
[0093] 3) Cement mortar filling;
[0094] 4) applying the epoxy interface agent prepared in Example 1;
[0095] 5) Lay the first layer of steel bars and set the upper and lower layer steel bar tie embedded parts;
[0096] 6) pouring concrete outer page to obtain outer page layer;
[0097] 7) Laying the insulation layer;
[0098] 8) Lay the second layer of steel bars, connect the first and second layers of steel bars, and pre-embed water and electricity pipelines, hoisting parts, and connectors;
[0099] 9) Casting lightweight aggregate concrete inner wall layer;
[0100] 10) Wall demoulding, maintenance and acceptance.
[0101] Example 3 Preparation of assembled ancient building threshold wall B
[0102] Except that in step 2), when the facing brick layer is grooved, the cross-sectional shape of the groove is a rectangular structure, and the other preparation methods are the same.
[0103] Example 4 Preparation of assembled ancient building threshold wall C
[0104] Except that the facing brick layer is not grooved in step 2), the other preparation methods are the same.
[0105] Example 5 Preparation of assembled ancient building threshold wall D
[0106] Except that the interface agent used in step 4) is a common interface agent purchased on the market, the other preparation methods are the same.
[0107] Example 6 Preparation of assembled ancient building threshold wall E
[0108] Except that the facing brick layer is not grooved in step 2) and the interface agent used in step 4) is a common interface agent purchased on the market, the other preparation methods are the same.
[0109] Performance Testing
[0110] The assembled ancient building sill wall AE prepared in Examples 2-6 was subjected to hoisting and moving bonding strength tests and water and alkali resistance tests.
[0111] For the bonding strength, it mainly depends on whether there are obvious cracks or even complete cracks during the lifting and moving process. The water resistance and alkali resistance are to observe whether the interface layer is obviously whitened or bubbling after the wall is stored for three months. The specific performance results of the test side are shown in Table 1
[0112] Table 1 Performance test results of prefabricated ancient building sill wall
[0113] Example Threshold wall Bonding effect Water resistance Example 2 Prefabricated ancient building threshold wall A Excellent, no cracks good Example 3 Prefabricated ancient building threshold wall B Excellent, very few fine cracks good Example 4 Prefabricated ancient building threshold wall C Generally, there are a few cracks good Example 5 Prefabricated ancient building threshold wall D Generally, there are a few cracks Slight whitening Example 6 Prefabricated ancient building threshold wall E Failed, fell off Slight whitening
Claims
1. A method for preparing an assembled ancient building wall, characterized in that: The thickness of the wall of the prefabricated ancient building is 210-330 mm, and it includes a 30-50 mm thick brick layer, a 40-60 mm thick concrete outer page layer, a 60-100 mm thick insulation layer and an 80-120 mm thick concrete structural wall inner page layer from the outer wall to the inner wall, which includes the following steps: (1) Mold cleaning; (2) Arrange the bricks and fill the seams with sponge strips to obtain the facing brick layer, and make grooves on the side of the facing brick layer close to the outer layer of concrete; (3) Filling joints with cement mortar; (4) Applying an interface agent on the side of the tile layer close to the outer layer of the concrete; the interface agent is an epoxy interface agent, which is prepared by mixing component A and component B in a weight ratio range of (4-6):1, wherein component A comprises the following components in weight: 60-80 parts of epoxy acrylic resin, 10-20 parts of active diluent, 5-10 parts of auxiliary agent, 10-30 parts of conventional diluent A, and 20-30 parts of filler; component B comprises: 10-30 parts of amine curing agent and conventional diluent B; the auxiliary agent includes a wetting agent, a leveling agent, a defoaming agent, a dispersant, and an anti-settling agent; wherein the epoxy acrylic resin is prepared by free radical copolymerization of a first monomer, a second monomer, and a third monomer, wherein the first monomer is an acrylate monomer having three or more unsaturated carbon-carbon double bonds, the second monomer is a monomer having an unsaturated carbon-carbon double bond and an epoxy group, and the third monomer is γ-methacryloxypropyltrimethoxysilane; (5) Lay the first layer of steel bars and install the upper and lower layer steel bar tie embedded parts; (6) pouring concrete to obtain an outer concrete layer; (7) Laying the insulation layer; (8) Lay the second layer of steel bars, connect the first layer of steel bars with the second layer of steel bars, and pre-embed water and electricity pipelines, lifting parts, and connectors; (9) Casting the inner layer of the concrete structure wall; (10) Wall demoulding, maintenance and acceptance.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the first monomer, the second monomer and the third monomer is 2:(4-6):(0.4-0.6).
3. The preparation method according to claim 1, characterized in that: The amine curing agent is selected from triethylenetetramine, polyamide, polyetheramine and / or γ-aminopropyltriethoxysilane KH550.
4. The preparation method according to claim 1 or 3, characterized in that: The amine curing agent is a mixture of polyamide and γ-aminopropyltriethoxysilane, wherein the mass ratio of polyamide to γ-aminopropyltriethoxysilane is (8-10):
1.
5. The preparation method according to claim 1, characterized in that: The active diluent is 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, fatty glycidyl ether and / or butyl glycidyl ether; the conventional diluent A is xylene, butyl acetate, propylene glycol methyl ether acetate, ethylene glycol methyl ether, ethylene glycol butyl ether, acetone, butanone and / or cyclohexanone; the conventional diluent B is xylene, butyl acetate, propylene glycol methyl ether acetate, butanol, butanone, cyclohexanone and / or isopropanol.
6. The preparation method according to claim 1, characterized in that: The cross-sectional shape of the groove is square, rectangular or trapezoidal.
7. The preparation method according to claim 1, characterized in that: The facing brick layer is made of small mud bricks.
8. The preparation method according to claim 1, characterized in that: The wall is a sill wall, a gable wall or a rear eaves wall; the insulation material of the insulation layer is a molded polystyrene board, an extruded polystyrene board or a foamed polystyrene board.
Citation Information
Patent Citations
Interface agent, as well as preparation method and application thereof
CN104650302A
Sandwich heat preservation laminated shear wall and connecting piece
CN114135048A
Fabricated pseudo-classic building thermal insulation wall structure and using method thereof
CN115584805A
Novel thermal insulation brick and production method thereof
CN101008280A
Adhesive compound containing epoxy resin
CN101591466A