A kind of PET core material and preparation method thereof

By chemically and physically modifying PET materials, chain extension and blending technology are used to form a stable crosslinked structure, and the internal structure of polyester is optimized through heat treatment, which solves the problem of poor mechanical properties caused by low crystallinity of PET materials, significantly improving resistance Impact performance and thermal stability optimize the mechanical properties, especially in low temperature environments, showing good toughening effect.

CN118185116BActive Publication Date: 2024-11-15中威航空材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410450137.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-11-15
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

PET materials have low crystallinity during the continuous foaming process of industrial melting, resulting in poor mechanical properties and mechanical stability of the products. The existing foam core materials have low bonding strength, poor heat resistance, poor chemical resistance, low toughness and fatigue resistance. Difference.

Method used

Modify PET materials through chemical and physical means, improve the comprehensive performance of PET materials by chain extension and blending, and premodify them using lysine methyl ester diisocyanate and calcium trifluoromethanesulfonate to form a stable Cross-linked and branched structures enhance the toughness and impact resistance of polyester, and optimize the internal structure of polyester through heat treatment to improve tensile strength and elongation of break.

Benefits of technology

It significantly improves the impact resistance, crystallization and thermal stability of the PET core material, optimizes the mechanical properties, including tensile strength and elongation at break, enhances the toughness and weather resistance of the material, especially in low temperature environments. Good toughening effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_15
    Figure SMS_15
Patent Text Reader

Abstract

The present invention belongs to the field of polymer synthesis, and in particular, relates to a PET core material and a preparation method thereof. The method comprises: (1) uniformly mixing cyclic carboxylic acid, acyclic alcohol, isocyanate derivative and acid-base balance regulator in proportion to prepare pre-modified polyethylene terephthalate; (2) uniformly mixing pre-modified polyethylene terephthalate, organic calcium and foaming agent in proportion, melting and stirring, cooling to room temperature, heat treating and curing to obtain polyethylene terephthalate core material, that is, PET core material. The present invention strengthens the impact resistance of PET core material by chemical grafting and chain extension, uses physical method of blending to change the crystallization performance and thermal stability of PET core material, and further heat treats the foamed polyester to reintegrate the internal structure of polyester, thereby optimizing the mechanical properties of PET core material, including optimizing tensile strength and elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer synthesis, and in particular relates to a PET core material and a preparation method thereof. Background Art

[0002] With the rapid development of science and technology, PET materials have shown broad application prospects in the field of fillers. PET materials, also known as polyethylene terephthalate, are linear thermoplastic resins with good weather resistance and chemical stability, impact resistance, maximum output, and the lowest price. However, in the process of industrial melt continuous foaming, due to the presence of rigid benzene rings in the PET molecular chain and the relatively short flexible carbon chain, its crystallization rate is slow, and the crystallinity is low during the melt cooling process, resulting in poor mechanical properties and mechanical stability of the product. In the existing public technical solutions, each foam has different properties due to different materials and molding processes, which will directly affect the performance of the foam core material. The technical defects of the mainstream foam core materials on the market are low bonding strength with composite materials, poor material quality, poor heat resistance, poor chemical tolerance, low toughness, and poor fatigue resistance.

[0003] In addition, the industrial production of PET foam materials in my country is still in its infancy, with only a few companies building production lines, and the product performance and variety are still somewhat behind those of foreign companies, and the market gap is still large. The preparation of PET foam materials with higher foaming ratios (>30 times) and the functional expansion of foam materials are still the key directions for future research. Summary of the invention

[0004] The technical solution of the present invention aims at the technical problems such as low crystallinity in the traditional melt cooling process, which leads to poor mechanical properties and mechanical stability of the product, and effectively improves the comprehensive performance of PET core material through chemical and physical means, and provides a method for preparing PET core material.

[0005] The main purpose of the present invention is:

[0006] 1. Strengthen the impact resistance of PET core material;

[0007] 2. Change the crystallization properties and thermal stability of PET core material;

[0008] 3. Optimize the mechanical properties of PET core materials, including tensile strength and elongation at break.

[0009] To achieve the above objectives, the present invention adopts the following technical solutions.

[0010] A method for preparing a PET core material,

[0011] The method comprises:

[0012] (1) mixing cyclic carboxylic acid, acyclic alcohol, isocyanate derivative and acid-base balance regulator in proportion to prepare pre-modified polyethylene terephthalate;

[0013] (2) Pre-modified polyethylene terephthalate, organic calcium and foaming agent are mixed uniformly in proportion, melted and stirred, cooled to room temperature, heat treated and solidified to obtain polyethylene terephthalate core material, that is, PET core material.

[0014] As a preference,

[0015] The cyclic carboxylic acid in step (1) is terephthalic acid;

[0016] The acyclic alcohol in step (1) is ethylene glycol;

[0017] The isocyanate derivative in step (1) is lysine methyl diisocyanate;

[0018] The acid-base balance regulator in step (1) is potassium carbonate.

[0019] As a preference,

[0020] In step (1), the cyclic carboxylic acid, acyclic alcohol, isocyanate derivative and acid-base balance regulator are uniformly mixed in a mass ratio of 4: (3.8-4.2): 2: (0.8-1.2).

[0021] As a preference,

[0022] The preparation of the pre-modified polyethylene terephthalate in step (1) is carried out under a nitrogen atmosphere at a temperature of 220 to 240° C. and a stirring rate of 600 to 1200 r / min for a continuous reaction of 6 to 10 hours.

[0023] As a preference,

[0024] The organic calcium in step (2) is calcium trifluoromethanesulfonate;

[0025] The foaming agent in step (2) is azodicarbonamide.

[0026] As a preference,

[0027] In step (2), the pre-modified polyethylene terephthalate, organic calcium and foaming agent are uniformly mixed in a mass ratio of 1: (0.6-1.0): (0.2-0.6).

[0028] As a preference,

[0029] The melting and stirring in step (2) is carried out under a nitrogen atmosphere at a temperature of 250-260° C. and a stirring rate of 600-1200 r / min for a continuous reaction of 2-4 h.

[0030] As a preference,

[0031] The heat treatment in step (2) is to raise the temperature to 200-220°C and keep it at that temperature for 30-60 minutes.

[0032] A PET core material.

[0033] In the technical solution of the present invention, the core lies in using chain extension and blending to improve the comprehensive performance of PET materials, especially maintaining good tensile properties in low temperature environments. The excellent performance of polyethylene terephthalate is mainly determined by the internal structure formed after curing. Therefore, if you want to improve and strengthen the mechanical properties of polyethylene terephthalate, you must reasonably change the arrangement of polyester macromolecules. The embrittlement and deterioration of stress-bearing properties of polyethylene terephthalate in low temperature environment are due to the highly cross-linked three-dimensional network structure formed after the polyethylene terephthalate is cured. On the one hand, the technical solution of the present invention first uses lysine methyl diisocyanate to extend the polyester chain, reduce the cross-linking effect between polyester molecules, eliminate the three-dimensional structure, and make the polyester molecules unfold in a two-dimensional plane to form a stable cross-linked and branched structure. Lysine methyl diisocyanate does not directly participate in the curing reaction after chain extension. At this time, the polyester macromolecules inside the core material are the continuous phase and the isocyanate is the dispersed phase. When this structure is subjected to external forces, the force will be evenly diffused throughout the core material, and no stress accumulation points will appear, which can hinder crack propagation and absorb energy. At the same time, the horizontal cross-linking of the polyester branches can reduce the cross-linking density of the polyethylene terephthalate long chain, increase the distance between the chain segments, and improve the toughness of the core material; on the other hand, through the trifluoroethylene The addition of calcium methanesulfonate is used for blending modification to improve the mechanical properties of polyethylene terephthalate. Through the compatibility of halogen with polyethylene terephthalate side chains, vertical anchor crosslinking is generated on the horizontal polyester molecular plane, hub crystallization is generated, and the torque of polyethylene terephthalate is strengthened. At the same time, the impact performance and elongation at break of the final core material are improved through copolymerization and in-situ reaction expansion between calcium and polyester long chains. When this structure is subjected to external forces, the continuous phase transmits the force to the crystallization, and the crystal deforms along the stretching direction to absorb energy, achieving a shock-absorbing effect. At this time, calcium trifluoromethanesulfonate is toughened by copolymerization, extending the polyester long chain with greater flexibility, and expanding the distance between crosslinking bonds after curing, increasing the range of chain segment movement, thereby improving the toughness of the PET core material. The special calcium salt restricts the isocyanate group on the polyester main chain through the growth of the lattice in a high temperature environment to cause branching or crosslinking reactions, thereby achieving a control effect on chain extension modification and its crosslinking degree.

[0034] Whether it is a crystalline or non-crystalline polymer material, under the influence of the external environment, the polymer chain will be arranged in parallel along the external field direction to form a stable orientation structure. The final polymer chain orientation has a significant effect on the performance of the polymer, is conducive to the crystallization process, and further affects its mechanical properties. In the technical solution of the present invention, another core is to perform heat treatment after foaming and curing. During the heat treatment process, the internal chain segments of the cured polyester are thawed, the internal stress generated during the foaming process is digested, and the generation of internal stress is reduced as much as possible by gradually and slowly cooling, so that stress concentration is not easy to occur inside the polyester core material. At the same time, the groups hindered by the steric hindrance effect during heat treatment are reacted, thereby optimizing the cross-linked network structure, thereby improving the strength. On the other hand, the internal space of the polyester is more finely arranged during the heat treatment process, and a core material with a smaller pore size is obtained, and the elongation at break is increased, thereby improving the overall performance of the core material. In addition, after heat treatment, the modified polyethylene terephthalate main chain and trifluoromethanesulfonic acid calcium salt produce a new chemical network structure, generating intramolecular holes, which can provide movement space for the segments and absorb a large amount of energy during the collision process.

[0035] The advantages of the present invention are:

[0036] (1) The present invention strengthens the impact resistance of PET core material by chemical grafting and chain extension;

[0037] (2) The present invention uses a physical method of blending to change the crystallization properties and thermal stability of the PET core material;

[0038] (3) In the technical solution of the present invention, the foamed polyester is heat-treated to reintegrate the internal structure of the polyester, thereby optimizing the mechanical properties of the PET core material, including optimizing the tensile strength and elongation at break. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0040] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0041] Embodiment 1: A method for preparing a PET core material,

[0042] The method comprises:

[0043] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, lysine methyl ester diisocyanate with a purity of 98%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:3.8:2:0.8, and reacted continuously for 10 hours at a temperature of 220°C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare pre-modified polyethylene terephthalate;

[0044] (2) Pre-modified polyethylene terephthalate, 99% pure calcium trifluoromethanesulfonic acid salt and azodicarbonamide were uniformly mixed in a mass ratio of 1:0.6:0.2, and melt-stirred for 4 h at a temperature of 250 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature, and then heated to 200 °C again and kept at this temperature for 60 min. The mixture was cooled and shaped to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0045] The PET core material prepared in the embodiment was tested, and the specific characterization results are as follows:

[0046] Fracture toughness test: The core material prepared in the embodiment is pre-cut with a blade to form a notch with an initial crack of 0.2 times its width, and then stretched at a strain rate of 0.008 / s, and the fracture toughness is calculated according to the following formula:

[0047] Where:

[0048] P——sample load;

[0049] A——Original cross-sectional area of ​​the sample, mm 2 ;

[0050] L——original gauge length of the sample, mm;

[0051] L0——Length of the sample after deformation, mm.

[0052] The load (P) refers to the external force and other factors that cause internal force and deformation in the structure or component. P = bulk density × thickness.

[0053] Cyclic tensile test: The core material prepared in the embodiment is made into an I-type dumbbell mold with reference to the sample size of GB / T2567-2008, and is continuously cycled at a loading speed of 5 mm / min and an unloading speed of 5 mm / min at room temperature until the elongation at break of the sample is exceeded to ductile fracture, and the tensile failure work is calculated according to the following formula:

[0054] Where:

[0055] L1——gage length after spline breaking, mm;

[0056] L0——the original gauge length of the spline, mm;

[0057] σ——cyclic stretching rate, mm / min;

[0058] A1——Minimum area of ​​the neck, mm 2 ;

[0059] A0——Original cross-sectional area of ​​the spline, mm 2 ;

[0060] σ'——unloading rate, mm / min.

[0061] The ratio of the energy loss during the spline failure to the tensile failure work (U n / W) represents the irreversible work generated by internal damage during stretching. The larger the ratio, the more serious the damage to the internal structure of the material. The energy loss of the spline during the destruction process can be calculated according to the following formula:

[0062] Where:

[0063] ε0——initial energy of the detection process, J;

[0064] ε n ——The dissipated energy after the nth test, J.

[0065] Low-temperature tensile properties: The core material prepared in the example was made into an I-type dumbbell mold with reference to the specimen size of GB / T2567-2008. The tensile properties were tested at a loading speed of 2 mm / min at -60°C, and the ultimate stress before the core material broke was recorded.

[0066] Impact performance: With reference to the impact strength test method of GB / T2567-2008, the core material prepared in the embodiment was made into the standard size of the impact specimen specified in the national standard, and then a pendulum was used to impact the middle of the core material with an impact energy of 1 J and an impact speed of 2.9 m / s. The energy of the impact loss was calculated by the deflection angle before and after the pendulum impact.

[0067] End carboxyl content detection: Dissolve 100 mg of PBT sample in 15 mL of phenol / 1,1,2,2-tetrachloroethane solution (v / v=3:2). Use bromothymol blue as an indicator and titrate with about 0.01 mol / L potassium hydroxide / methanol standard solution. The titration endpoint is blue and purple for at least 10 s, and the carboxyl end group content is calculated by the following formula:

[0068] Where:

[0069] CT——carboxyl end group content, mol / t;

[0070] V——consumption volume of potassium hydroxide / methanol standard solution, mL;

[0071] V0——consumption volume of potassium hydroxide / methanol standard solution of blank sample, mL;

[0072] N——potassium hydroxide / methanol standard solution concentration, mol / L;

[0073] G——sample mass, kg.

[0074]

[0075] Based on all the above characterization results, it is proved that the technical solution of the present invention not only has a reinforcing effect on the toughness and strength of PET materials under room temperature conditions, but also, compared with general materials, the toughness of the material will be greatly reduced at low temperatures, which is a very fatal defect for polyethylene terephthalate. However, the present invention has been modified by chemical and physical means, so that PET still has a good toughening effect under -60 ° C environment. At the same time, the more end group content in the polyester, the more flexible segments can be formed in the three-dimensional network after curing, the larger the spacing between the cross-linking points, and the greater the deformation can be generated when impacted to consume the impact energy.

[0076] Embodiment 2: A method for preparing a PET core material,

[0077] The method comprises:

[0078] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, lysine methyl ester diisocyanate with a purity of 98%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:4:2:1, and reacted continuously for 8 hours at a temperature of 230 °C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare pre-modified polyethylene terephthalate;

[0079] (2) Pre-modified polyethylene terephthalate, calcium trifluoromethanesulfonate with a purity of ≥99% and azodicarbonamide were uniformly mixed in a mass ratio of 1:0.8:0.4, and melt-stirred for 3 h at a temperature of 255 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature, and then heated to 210 °C again, kept at this temperature for 45 min, and cooled to shape to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0080] The PET core material prepared in the embodiment was tested, and the specific characterization results are as follows:

[0081] Fracture toughness test: The core material prepared in the embodiment is pre-cut with a blade to form a notch with an initial crack of 0.2 times its width, and then stretched at a strain rate of 0.008 / s, and the fracture toughness is calculated according to the following formula:

[0082] Where:

[0083] P——sample load;

[0084] A——Original cross-sectional area of ​​the sample, mm 2 ;

[0085] L——original gauge length of the sample, mm;

[0086] L0——Length of the sample after deformation, mm.

[0087] The load (P) refers to the external force and other factors that cause internal force and deformation in the structure or component. P = bulk density × thickness.

[0088] Cyclic tensile test: The core material prepared in the embodiment is made into an I-type dumbbell mold with reference to the sample size of GB / T2567-2008, and is continuously cycled at a loading speed of 5 mm / min and an unloading speed of 5 mm / min at room temperature until the elongation at break of the sample is exceeded to ductile fracture, and the tensile failure work is calculated according to the following formula:

[0089] Where:

[0090] L1——gage length after spline breaking, mm;

[0091] L0——the original gauge length of the spline, mm;

[0092] σ——cyclic stretching rate, mm / min;

[0093] A1——Minimum area of ​​the neck, mm 2 ;

[0094] A0——Original cross-sectional area of ​​the spline, mm 2 ;

[0095] σ'——unloading rate, mm / min.

[0096] The ratio of the energy loss during the spline failure to the tensile failure work (U n / W) represents the irreversible work generated by internal damage during stretching. The larger the ratio, the more serious the damage to the internal structure of the material. The energy loss of the spline during the destruction process can be calculated according to the following formula:

[0097] Where:

[0098] ε0——initial energy of the detection process, J;

[0099] ε n ——The dissipated energy after the nth test, J.

[0100] Low-temperature tensile properties: The core material prepared in the example was made into an I-type dumbbell mold with reference to the specimen size of GB / T2567-2008. The tensile properties were tested at a loading speed of 2 mm / min at -60°C, and the ultimate stress before the core material broke was recorded.

[0101] Impact performance: With reference to the impact strength test method of GB / T2567-2008, the core material prepared in the embodiment was made into the standard size of the impact specimen specified in the national standard, and then a pendulum was used to impact the middle of the core material with an impact energy of 1 J and an impact speed of 2.9 m / s. The energy of the impact loss was calculated by the deflection angle before and after the pendulum impact.

[0102] End carboxyl content detection: Dissolve 100 mg of PBT sample in 15 mL of phenol / 1,1,2,2-tetrachloroethane solution (v / v=3:2). Use bromothymol blue as an indicator and titrate with about 0.01 mol / L potassium hydroxide / methanol standard solution. The titration endpoint is blue and purple for at least 10 s, and the carboxyl end group content is calculated by the following formula:

[0103] Where:

[0104] CT——carboxyl end group content, mol / t;

[0105] V——consumption volume of potassium hydroxide / methanol standard solution, mL;

[0106] V0——consumption volume of potassium hydroxide / methanol standard solution of blank sample, mL;

[0107] N——potassium hydroxide / methanol standard solution concentration, mol / L;

[0108] G——sample mass, kg.

[0109]

[0110] Embodiment 3: A method for preparing a PET core material,

[0111] The method comprises:

[0112] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, lysine methyl ester diisocyanate with a purity of 98%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:4.2:2:1.2, and reacted continuously for 6 hours at a temperature of 240°C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare pre-modified polyethylene terephthalate;

[0113] (2) Pre-modified polyethylene terephthalate, 99% pure calcium trifluoromethanesulfonic acid salt and azodicarbonamide were uniformly mixed in a mass ratio of 1:1.0:0.6, and melt-stirred for 2 h at a temperature of 260 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature, and then heated to 220 °C again and kept at this temperature for 30 min. The mixture was cooled and shaped to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0114] The PET core material prepared in the embodiment was tested, and the specific characterization results are as follows:

[0115] Fracture toughness test: The core material prepared in the embodiment is pre-cut with a blade to form a notch with an initial crack of 0.2 times its width, and then stretched at a strain rate of 0.008 / s, and the fracture toughness is calculated according to the following formula:

[0116] Where:

[0117] P——sample load;

[0118] A——Original cross-sectional area of ​​the sample, mm 2 ;

[0119] L——original gauge length of the sample, mm;

[0120] L0——Length of the sample after deformation, mm.

[0121] The load (P) refers to the external force and other factors that cause internal force and deformation in the structure or component. P = bulk density × thickness.

[0122] Cyclic tensile test: The core material prepared in the embodiment is made into an I-type dumbbell mold with reference to the sample size of GB / T2567-2008, and is continuously cycled at a loading speed of 5 mm / min and an unloading speed of 5 mm / min at room temperature until the elongation at break of the sample is exceeded to ductile fracture, and the tensile failure work is calculated according to the following formula:

[0123] Where:

[0124] L1——gage length after spline breaking, mm;

[0125] L0——the original gauge length of the spline, mm;

[0126] σ——cyclic stretching rate, mm / min;

[0127] A1——Minimum area of ​​the neck, mm 2 ;

[0128] A0——Original cross-sectional area of ​​the spline, mm 2 ;

[0129] σ'——unloading rate, mm / min.

[0130] The ratio of the energy loss during the spline failure to the tensile failure work (U n / W) represents the irreversible work generated by internal damage during stretching. The larger the ratio, the more serious the damage to the internal structure of the material. The energy loss of the spline during the destruction process can be calculated according to the following formula:

[0131] Where:

[0132] ε0——initial energy of the detection process, J;

[0133] ε n ——The dissipated energy after the nth test, J.

[0134] Low-temperature tensile properties: The core material prepared in the example was made into an I-type dumbbell mold with reference to the specimen size of GB / T2567-2008. The tensile properties were tested at a loading speed of 2 mm / min at -60°C, and the ultimate stress before the core material broke was recorded.

[0135] Impact performance: With reference to the impact strength test method of GB / T2567-2008, the core material prepared in the embodiment was made into the standard size of the impact specimen specified in the national standard, and then a pendulum was used to impact the middle of the core material with an impact energy of 1 J and an impact speed of 2.9 m / s. The energy of the impact loss was calculated by the deflection angle before and after the pendulum impact.

[0136] End carboxyl content detection: Dissolve 100 mg of PBT sample in 15 mL of phenol / 1,1,2,2-tetrachloroethane solution (v / v=3:2). Use bromothymol blue as an indicator and titrate with about 0.01 mol / L potassium hydroxide / methanol standard solution. The titration endpoint is blue and purple for at least 10 s, and the carboxyl end group content is calculated by the following formula:

[0137] Where:

[0138] CT——carboxyl end group content, mol / t;

[0139] V——consumption volume of potassium hydroxide / methanol standard solution, mL;

[0140] V0——consumption volume of potassium hydroxide / methanol standard solution of blank sample, mL;

[0141] N——potassium hydroxide / methanol standard solution concentration, mol / L;

[0142] G——sample mass, kg.

[0143]

[0144] Comparative Example 1: A method for preparing a PET core material, wherein the specific preparation method is the same as that of Example 2, except that the trifluoromethanesulfonic acid calcium salt unique to the present invention is not used, and the PET core material is prepared. The specific operation is as follows:

[0145] A method for preparing a PET core material,

[0146] The method comprises:

[0147] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, lysine methyl ester diisocyanate with a purity of 98%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:4:2:1, and reacted continuously for 8 hours at a temperature of 230 °C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare pre-modified polyethylene terephthalate;

[0148] (2) Pre-modified polyethylene terephthalate and azodicarbonamide were uniformly mixed in a mass ratio of 1:0.4, and melt-stirred for 3 h at a temperature of 255 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature and fixed to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0149] The PET core material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0150]

[0151] By comparing the above characterization results with Example 2, it is found that the terminal carboxyl content in the PET core material prepared in the comparative example is significantly improved. The inventor originally predicted that with the increase of the terminal carboxyl content, the fracture toughness and impact strength of the core material should be improved. However, after observation of the comparative example, with the excessive increase of the terminal carboxyl content, the cross-linking structure density inside the core material decreases, and there is no anchoring of calcium trifluoromethanesulfonic acid salt between the polyester molecular chains, which increases the intermolecular distance, reduces the intermolecular force, and enhances the activity of the chain segments, which in turn leads to a decrease in fracture toughness and impact strength.

[0152] Comparative Example 2 is a method for preparing a PET core material. The specific preparation method is the same as that of Example 2, except that the lysine methyl ester diisocyanate unique to the present invention is not used to prepare the PET core material. The specific operation is as follows:

[0153] A method for preparing a PET core material,

[0154] The method comprises:

[0155] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:4:1, and reacted continuously for 8 hours at a temperature of 230 °C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare polyethylene terephthalate;

[0156] (2) Pre-modified polyethylene terephthalate, trifluoromethanesulfonic acid calcium salt with a purity of ≥99% and azodicarbonamide were uniformly mixed in a mass ratio of 1:0.8:0.4, and melt-stirred for 3 h at a temperature of 255 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature and fixed to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0157] The PET core material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0158]

[0159] By comparing the above characterization results with those of Example 2, it is found that the PET core material prepared in the comparative example has a significant decrease in cyclic tensile properties and low-temperature tensile properties. The inventors have found that in the technical scheme of the present invention, lysine methyl ester diisocyanate not only acts as a chemical chain extender, but also plays a role in chemical nucleation, reducing the free energy of the polyester molecular chain entering the trifluoromethanesulfonic acid calcium salt crystal, while also increasing the growth rate of the trifluoromethanesulfonic acid calcium salt crystal nucleus, compensating for the decrease in molecular weight caused by the addition of trifluoromethanesulfonic acid calcium salt, and improving the tensile strength of the core material after foaming.

[0160] Comparative Example 3: A method for preparing a PET core material. The specific preparation method is the same as that of Example 2, except that the lysine methyl ester diisocyanate unique to the present invention is replaced with an equal amount of oxidized bis(4-phenylisocyanate) to prepare the PET core material. The specific operation is as follows:

[0161] A method for preparing a PET core material,

[0162] The method comprises:

[0163] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, bis(4-phenylisocyanate) oxide with a purity of 98%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:4:2:1, and the mixture was reacted continuously for 8 hours at a temperature of 230 °C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare pre-modified polyethylene terephthalate;

[0164] (2) Pre-modified polyethylene terephthalate, trifluoromethanesulfonic acid calcium salt with a purity of ≥99% and azodicarbonamide were uniformly mixed in a mass ratio of 1:0.8:0.4, and melt-stirred for 3 h at a temperature of 255 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature and fixed to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0165] The PET core material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0166]

[0167] By comparing the above characterization results with those of Example 2, it is found that the core material prepared in the comparative example has extremely high fracture toughness and resistance to tensile damage, but structural defects appear inside the core material, and the tensile properties in a low-temperature environment are significantly reduced. The inventors have found that the main chain of the internal skeleton of the PET substrate modified with oxidized bis(4-phenylisocyanate) undergoes significant changes, and the skeleton is full of polyester chain bonds and unsaturated double bonds. The polyester has a carboxyl group and an isocyanate group at both ends. In a low-temperature environment, due to the high cross-linking density of the unsaturated groups, the core material performance will show a brittle transition, and the elongation at break will decrease. At this time, when the core material is subjected to external forces, the elastic stress inside the core material accumulates rapidly under the condition of local structural loss, which accelerates the structural collapse of the core material in a low-temperature environment.

[0168] Comparative Example 4: A method for preparing a PET core material, wherein the specific preparation method is the same as that of Example 2, except that the heat treatment unique to the present invention is not used, and the PET core material is prepared. The specific operation is as follows:

[0169] A method for preparing a PET core material,

[0170] The method comprises:

[0171] (1) Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, lysine methyl ester diisocyanate with a purity of 98%, and potassium carbonate with a purity of 99% were uniformly mixed in a mass ratio of 4:4:2:1, and reacted continuously for 8 hours at a temperature of 255 °C and a stirring rate of 900 r / min under a nitrogen atmosphere to prepare pre-modified polyethylene terephthalate;

[0172] (2) Pre-modified polyethylene terephthalate, trifluoromethanesulfonic acid calcium salt with a purity of ≥99% and azodicarbonamide were uniformly mixed in a mass ratio of 1:0.8:0.4, and melt-stirred for 3 h at a temperature of 280 °C and a stirring rate of 900 r / min under a nitrogen atmosphere. The mixture was cooled to room temperature and fixed to obtain a polyethylene terephthalate core material, i.e., a PET core material.

[0173] The PET core material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0174]

[0175] In addition, a special test was performed on Example 2 and the comparative example. In the same natural environment and test method, the bending strength of the core material prepared in Example 2 and the core material prepared in the comparative example was measured, and the following formula was used to calculate whether the core material had notch sensitivity:

[0176] Where:

[0177] σ1——bending strength of notch test sample, MPa;

[0178] σ2——Bending strength of unnotched test specimen, MPa.

[0179] By comparing the above characterization results with those of Example 2, it is found that the performance of the core material prepared in the comparative example is reduced, and after special testing, it is found that the comparative example core material produces notch sensitivity. The inventors have found that if a higher temperature is used in the foaming process in the technical scheme of the present invention, the foaming agent and the metal crystals inside the PET material produce non-directional alternating jumps, deform in an unstable manner, and cracks appear in the expansion process, and impact fractures appear, resulting in the superposition of unevenness, resulting in unstable nodes in the internal structure of the PET core material.

[0180] Comparative Example 5: A commercially available PET filling core material was characterized by the same performance as that of Example 2. The specific characterization results are as follows.

[0181]

[0182] By comparing the above characterization results with Example 2, it is found that the commercially available filling core material has stronger fracture toughness and tensile resistance. However, the core material provided by the present invention is more stable inside and is not prone to internal structural damage during the cyclic stretching process. At the same time, it can maintain high tensile properties in a low temperature environment, achieving good kinetic energy absorption and shock absorption effects.

Claims

1. A method for preparing a PET core material, It is characterized in that The method comprises: (1) mixing cyclic carboxylic acid, acyclic alcohol, isocyanate derivative and acid-base balance regulator in proportion to prepare pre-modified polyethylene terephthalate; (2) Pre-modified polyethylene terephthalate, organic calcium and foaming agent are uniformly mixed in proportion, melted and stirred, cooled to room temperature, heat treated and solidified to obtain polyethylene terephthalate core material, that is, PET core material; The cyclic carboxylic acid in step (1) is terephthalic acid; The acyclic alcohol in step (1) is ethylene glycol; The isocyanate derivative in step (1) is lysine methyl diisocyanate; The organic calcium in step (2) is calcium trifluoromethanesulfonate; The heat treatment in step (2) is to raise the temperature to 200-220°C and keep it at that temperature for 30-60 minutes.

2. A method for preparing a PET core material according to claim 1, It is characterized in that The acid-base balance regulator in step (1) is potassium carbonate.

3. A method for preparing a PET core material according to claim 1 or 2, It is characterized in that In step (1), the cyclic carboxylic acid, acyclic alcohol, isocyanate derivative and acid-base balance regulator are uniformly mixed in a mass ratio of 4: (3.8-4.2): 2: (0.8-1.2).

4. A method for preparing a PET core material according to claim 1, It is characterized in that The preparation of the pre-modified polyethylene terephthalate in step (1) is carried out under a nitrogen atmosphere at a temperature of 220 to 240°C and a stirring rate of 600 to 1200 r / min for a continuous reaction of 6 to 10 hours.

5. A method for preparing a PET core material according to claim 1, It is characterized in that The foaming agent in step (2) is azodicarbonamide.

6. A method for preparing a PET core material according to claim 1 or 5, It is characterized in that In step (2), the pre-modified polyethylene terephthalate, organic calcium and foaming agent are uniformly mixed in a mass ratio of 1: (0.6-1.0): (0.2-0.6).

7. A method for preparing a PET core material according to claim 1, It is characterized in that The melt stirring in step (2) is carried out under a nitrogen atmosphere at a temperature of 250-260°C and a stirring rate of 600-1200 r / min for a continuous reaction of 2-4 h.

8. A PET core material obtained by the method according to any one of claims 1 to 7.