A weather-resistant polypropylene composite material for new energy battery shell and preparation method thereof

By adding polypropylene grafted glycidyl methacrylate and hindered phenol-based antioxidant flame retardant to the polypropylene composite material, a phosphorus-silicon flame retardant system is formed, which solves the problem of poor flame retardancy of polypropylene in the lithium battery casing of new energy vehicles. problem, significantly improving its flame retardant performance and safety performance, and is suitable for new energy vehicle battery casings.

CN118185180BActive Publication Date: 2024-10-15广东亨嘉橡塑科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410388263.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-01
Publication Date
2024-10-15
Estimated Expiration
2044-04-01

AI Technical Summary

Technical Problem

Polypropylene has problems with poor flame retardancy and poor heat and weather resistance in new energy vehicle lithium battery casings, resulting in insufficient safety performance.

Method used

A weather-resistant polypropylene composite material is used. By adding polypropylene grafted with glycidyl methacrylate and hindered phenol-based antioxidant flame retardant, a phosphorus-silicon flame retardant system is formed to improve the compatibility and flame retardant properties of the polypropylene resin. , and materials with excellent flame retardant properties are prepared through a twin-screw extruder.

Benefits of technology

Significantly improves the combustion limit oxygen index of polypropylene to 27.4-30.2%, reaching UL-94 fire rating V-0, enhances the flame retardant performance and safety performance of polypropylene, and expands its application in new energy vehicle battery casings .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004771442370000031
    Figure BDA0004771442370000031
  • Figure BDA0004771442370000032
    Figure BDA0004771442370000032
  • Figure BDA0004771442370000051
    Figure BDA0004771442370000051
Patent Text Reader

Abstract

The invention relates to the technical field of polypropylene, and discloses a weather-resistant polypropylene composite material for a new energy battery shell and a preparation method thereof. The biphosphate structure and the siloxane structure in the molecular main chain of a hindered phenol-based antioxidant flame retardant form a phosphorus-silicon flame retardant system, and polypropylene grafted glycidyl methacrylate is added as a compatibilizer, and the epoxy group thereof reacts with the terminal amino group and the carboxyl group of the hindered phenol-based antioxidant flame retardant, thereby improving the compatibility between the hindered phenol-based antioxidant flame retardant and the polypropylene resin, making the hindered phenol-based antioxidant flame retardant uniformly dispersed in a polypropylene resin matrix, significantly improving the limiting oxygen index, thermal oxidation resistance and weather resistance of polypropylene combustion, and after accelerated thermal oxidation aging experiments, the notched impact strength of the polypropylene decreases very little, the polypropylene can be well applied to the battery shell of a new energy vehicle, has high impact strength, good mechanical properties, is not easy to expand and bulge, and has good safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polypropylene, and in particular to a weather-resistant polypropylene composite material for a new energy battery shell and a preparation method thereof. Background Art

[0002] At present, the batteries of new energy vehicles are mainly lithium batteries, which have the advantages of fast charging and discharging speed, large specific capacity, and green environmental protection. However, lithium batteries used in new energy vehicles may expand, bulge, and spontaneously combust, which are very harmful after burning. Developing battery casings with good weather resistance, high flame retardancy, and high mechanical strength can effectively improve the safety performance of lithium batteries.

[0003] At present, the shell of lithium battery is mainly made of plastics such as polypropylene and polyvinyl chloride. Among them, polypropylene is non-toxic and odorless, cheap and easy to obtain, and has been processed and formed. It is widely used in the fields of new energy vehicle battery shells, but polypropylene has poor flame retardancy and poor heat and weather resistance at high temperatures. CN113603962B discloses the use of high-impact polypropylene, toughening agent, pyrophosphate piperazine flame retardant, hyperbranched polyamide ester and other raw materials to prepare a high-toughness V0-level flame-retardant polypropylene composite material for battery shells. The halogen-free flame retardant is prevented from agglomerating by adding a hyperdispersant; however, the raw materials of this patent are relatively large, and the preparation method is complicated, which is not conducive to practical development and application. Summary of the invention

[0004] The technical problems solved are as follows: providing a weather-resistant polypropylene composite material, solving the problems of poor heat resistance, weather resistance and flame retardancy of polypropylene; and expanding the practical application of polypropylene in new energy vehicle battery casings.

[0005] The technical solution is as follows:

[0006] A weather-resistant polypropylene composite material comprises the following components in parts by weight: 87-98 parts of polypropylene resin, 0.3-2.5 parts of polypropylene grafted glycidyl methacrylate, 1-8 parts of hindered phenol-based antioxidant flame retardant, and 0.5-2 parts of lubricant.

[0007] The hindered phenol-based antioxidant flame retardant was prepared as follows: N-methylpyrrolidone, tartrate-based hindered phenol were added to the reaction bottle. Tartaric acid dimethyl phosphate 1,3-Bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane After stirring, pyridine and triphenyl phosphite are added, nitrogen is introduced, and the mixture is reacted at a temperature of 100-125° C. for 2-5 hours. After cooling, the solution is poured into a methanol aqueous solution, the precipitate is precipitated, filtered, and washed with ethanol to obtain a hindered phenol-based antioxidant flame retardant.

[0008] Preferably, the ratio of tartrate hindered phenol, tartrate dimethyl phosphate and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is (0.2-0.5):(0.5-0.8):1.

[0009] Preferably, the preparation method of tartrate hindered phenol is as follows: add N,N-dimethylformamide, D,L-tartaric acid, 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and triethylamine to a reaction bottle, add ethyl acetate and water after the reaction, extract and separate, dry the organic phase, concentrate and recrystallize to obtain tartrate hindered phenol. The reaction route is as follows:

[0010]

[0011] Preferably, the molar ratio of D,L-tartaric acid, 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and triethylamine is 1:(2-2.2):(1.8-2.3).

[0012] Preferably, the reaction is first carried out at room temperature for 6-12 hours, and then the temperature is raised to 55-65° C. for 4-8 hours.

[0013] Preferably, the preparation method of tartaric acid dimethyl phosphate is as follows: add any solvent selected from acetone, tetrahydrofuran, ethyl acetate, acetonitrile, D, L-tartaric acid, O, O-dimethylphosphoryl chloride, and triethylamine to a reaction bottle, react, concentrate the solvent, and recrystallize from ethanol to obtain tartaric acid dimethyl phosphate. The reaction route is as follows:

[0014]

[0015] Preferably, the molar ratio of D,L-tartaric acid, O,O-dimethylphosphoryl chloride and triethylamine is 1:(2-2.4):(2-2.6).

[0016] Preferably, the reaction is first carried out at 0-10°C for 0.5-1 h, and then the temperature is raised to 25-40°C for 6-18 h.

[0017] Preferably, the preparation method of the weather-resistant polypropylene composite material is as follows: 87-98 parts of polypropylene resin, 0.3-2.5 parts of polypropylene grafted glycidyl methacrylate, 1-8 parts of hindered phenol-based antioxidant flame retardant, and 0.5-2 parts of lubricant are added to a twin-screw extruder, the screw speed is 30-80r / min, the melt temperature is 180-190°C, and extrusion granulation is performed to obtain a weather-resistant polypropylene composite material.

[0018] Preferably, the weather-resistant polypropylene composite material is used in the battery casing of new energy vehicles.

[0019] The technical effects are as follows: The present invention prepares a novel tartrate-based hindered phenol containing a bis-hindered phenol structure and a tartaric acid-based dimethyl phosphate with a bis-phosphate structure, and then carries out an amidation copolymerization reaction with 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to obtain a novel hindered phenol-based antioxidant flame retardant.

[0020] The double phosphate structure and the siloxane structure in the main chain of the molecule of the hindered phenol-based antioxidant flame retardant of the present invention form a phosphorus-silicon flame retardant system, and the added polypropylene-grafted glycidyl methacrylate is used as a compatibilizer, and the epoxy group thereof reacts with the terminal amino group and the carboxyl group of the hindered phenol-based antioxidant flame retardant, thereby improving the compatibility between the hindered phenol-based antioxidant flame retardant and the polypropylene resin, making the hindered phenol-based antioxidant flame retardant uniformly dispersed in the polypropylene resin matrix, significantly improving the limiting oxygen index of polypropylene combustion to 27.4-30.2%, and the UL-94 fire protection grade reaches V-0 grade, having excellent flame retardant performance and safety performance, and expanding the practical application of polypropylene in the fields of battery shells of new energy vehicles.

[0021] The main chain of the hindered phenol-based antioxidant flame retardant of the present invention contains a flexible organosiloxane structure, which has a good toughening effect on polypropylene and significantly improves the notched impact strength. In addition, it contains a double hindered phenol structure, which can correct the peroxy radicals, hydroxyl radicals, etc. generated during the thermal oxidation aging of polypropylene, inhibit the thermal oxidation aging reaction process, thereby improving the thermal oxidation resistance and weather resistance of polypropylene. After accelerated thermal oxidation aging experiments, the notched impact strength of polypropylene decreases very little. It can be well applied to the battery shell of new energy vehicles, has high impact strength, good mechanical properties, is not easy to expand and bulge, and has good safety performance. DETAILED DESCRIPTION

[0022] The main raw materials of the present invention are:

[0023] D,L-Tartaric acid, CAS No. 133-37-9.

[0024] 3,5-Bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, CAS No. 3062-64-4, structural formula:

[0025]

[0026] O,O-Dimethylphosphoryl chloride, CAS No. 813-77-4. The structural formula is

[0027] 1,3-Bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, CAS No. 2469-55-8. The structural formula is

[0028] 50g of polypropylene, 5g of glycidyl methacrylate and 0.04g of diisopropylbenzene peroxide were added into a twin-screw extruder for melt grafting at 160°C for 8min. The product was dissolved in xylene, precipitated by adding acetone, filtered and washed with acetone to obtain polypropylene grafted with glycidyl methacrylate.

[0029] Example 1

[0030] Add 25 mL of N,N-dimethylformamide, 3 mmol of D,L-tartaric acid, 6 mmol of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and 6.9 mmol of triethylamine to the reaction bottle, first react at room temperature for 6 hours, then heat to 55°C and react for 6 hours, add ethyl acetate and water, extract and separate, dry the organic phase, concentrate and recrystallize to obtain tartrate-based hindered phenol.

[0031] Add acetone solvent, 2 mmol D,L-tartaric acid, 4 mmol O,O-dimethylphosphoryl chloride, and 4.5 mmol triethylamine to the reaction bottle, first react at 0°C for 1 hour, then heat to 25°C, react for 18 hours, concentrate the solvent, and recrystallize with ethanol to obtain tartaric acid dimethyl phosphate.

[0032] Add 30 mL of N-methylpyrrolidone, 2 mmol of tartrate-based hindered phenol, 8 mmol of tartrate-based dimethyl phosphate, and 10 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane into the reaction bottle, stir, add 30 mmol of pyridine and 12 mmol of triphenyl phosphite, introduce nitrogen, react at 100 ° C for 5 hours, cool, pour the solution into a methanol aqueous solution, precipitate, filter, and wash with ethanol to obtain a hindered phenol-based antioxidant flame retardant.

[0033] 980g of polypropylene resin, 3g of polypropylene grafted glycidyl methacrylate, 10 parts of hindered phenol-based antioxidant flame retardant, and 5g of lubricant polypropylene wax were added into a twin-screw extruder with a screw speed of 80r / min and a melting temperature of 180°C, and extrusion granulation was performed to obtain a weather-resistant polypropylene composite material.

[0034] Example 2

[0035] Add 25 mL of N,N-dimethylformamide, 3 mmol of D,L-tartaric acid, 6.6 mmol of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and 5.4 mmol of triethylamine to the reaction bottle, first at room temperature for 6 hours, then heat to 60°C and react for 4 hours, add ethyl acetate and water, extract and separate, dry the organic phase, concentrate and recrystallize to obtain tartrate-based hindered phenol.

[0036] Add acetonitrile solvent, 2 mmol D,L-tartaric acid, 4.8 mmol O,O-dimethylphosphoryl chloride, and 5.2 mmol triethylamine to the reaction bottle, first react at 10°C for 0.5 h, then heat to 25°C, react for 18 h, concentrate the solvent, and recrystallize with ethanol to obtain tartaric acid dimethyl phosphate.

[0037] Add 50 mL of N-methylpyrrolidone, 3 mmol of tartrate-based hindered phenol, 7 mmol of tartrate-based dimethyl phosphate, and 10 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane into the reaction bottle, stir, add 30 mmol of pyridine and 10 mmol of triphenyl phosphite, introduce nitrogen, react at 125 ° C for 5 hours, cool, pour the solution into a methanol-water solution, precipitate, filter, and wash with ethanol to obtain a hindered phenol-based antioxidant flame retardant.

[0038] 930 g of polypropylene resin, 12 g of polypropylene grafted glycidyl methacrylate, 45 parts of hindered phenol-based antioxidant flame retardant, and 10 g of lubricant polyethylene wax were added into a twin-screw extruder with a screw speed of 80 r / min and a melting temperature of 180° C., and extrusion granulation was performed to obtain a weather-resistant polypropylene composite material.

[0039] Example 3

[0040] Add 40 mL of N,N-dimethylformamide, 3 mmol of D,L-tartaric acid, 6.6 mmol of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and 6.9 mmol of triethylamine to the reaction bottle, first react at room temperature for 6 hours, then heat to 65°C and react for 4 hours, add ethyl acetate and water, extract and separate, dry the organic phase, concentrate and recrystallize to obtain tartrate-based hindered phenol.

[0041] Ethyl acetate solvent, 2 mmol D,L-tartaric acid, 4.4 mmol O,O-dimethylphosphoryl chloride, and 4 mmol triethylamine were added to the reaction bottle, and the mixture was first reacted at 0°C for 1 h, then the temperature was raised to 40°C and the reaction was continued for 6 h. The solvent was concentrated and recrystallized from ethanol to obtain tartaric acid dimethyl phosphate.

[0042] Add 50 mL of N-methylpyrrolidone, 5 mmol of tartrate-based hindered phenol, 5 mmol of tartrate-based dimethyl phosphate, and 10 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane into the reaction bottle, stir, add 35 mmol of pyridine and 10 mmol of triphenyl phosphite, introduce nitrogen, react at 110°C for 2 h, cool, pour the solution into a methanol-water solution, precipitate, filter, and wash with ethanol to obtain a hindered phenol-based antioxidant flame retardant.

[0043] 870g of polypropylene resin, 25g of polypropylene grafted glycidyl methacrylate, 80 parts of hindered phenol-based antioxidant flame retardant, and 20g of lubricant polyethylene wax were added into a twin-screw extruder with a screw speed of 30r / min and a melting temperature of 190°C, and extrusion granulation was performed to obtain a weather-resistant polypropylene composite material.

[0044] Comparative Example 1

[0045] 980g of polypropylene resin, 3g of polypropylene grafted glycidyl methacrylate, 10 parts of hindered phenol-based antioxidant flame retardant, and 5g of lubricant polypropylene wax were added into a twin-screw extruder with a screw speed of 80r / min and a melting temperature of 180°C, and extrusion granulation was performed to obtain a weather-resistant polypropylene composite material.

[0046] Comparative Example 2

[0047] 980 g of polypropylene resin, 10 parts of hindered phenol-based antioxidant flame retardant, and 5 g of lubricant polypropylene wax were added into a twin-screw extruder, the screw speed was 80 r / min, the melting temperature was 180° C., and extrusion granulation was performed to obtain a weather-resistant polypropylene composite material.

[0048] Comparative Example 3

[0049] 980g of polypropylene resin, 10 parts of hindered phenol antioxidant 1076 and 5g of lubricant polypropylene wax were added into a twin-screw extruder with a screw speed of 80r / min and a melting temperature of 180°C, and extruded and granulated to obtain a weather-resistant polypropylene composite material.

[0050] The polypropylene composite material is injection molded by an injection molding machine to form a specimen.

[0051] The flame retardant properties of polypropylene composite material specimens were tested according to UL-94 fire rating and GB / T 2406.1-2008 standards.

[0052] Table 1 Flame retardant properties test of polypropylene composite materials

[0053] UL-94 fire rating Limiting oxygen index (%) Example 1 V-0 27.4 Example 2 V-0 28.9 Example 3 V-0 30.2 Comparative Example 1 V-2 21.6 Comparative Example 2 V-0 26.5 Comparative Example 3 V-2 21.9

[0054] Each embodiment uses tartrate-based hindered phenol, tartrate-based dimethyl phosphate, and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane for copolymerization to obtain a hindered phenol-based antioxidant flame retardant. The bisphosphate structure and the siloxane structure in the main chain of the molecule form a phosphorus-silicon flame retardant system, and the added polypropylene grafted methacrylate glycidyl ester is used as a compatibilizer. Its epoxy group reacts with the terminal amino group and carboxyl group of the hindered phenol-based antioxidant flame retardant, thereby improving the compatibility between the hindered phenol-based antioxidant flame retardant and the polypropylene resin, making it uniformly dispersed in the polypropylene resin matrix, significantly improving the limiting oxygen index of polypropylene combustion to 27.4-30.2%, and the UL-94 fire rating reaches V-0 level. It has excellent flame retardant properties and expands the practical application of polypropylene in the fields of new energy vehicle battery casings.

[0055] Comparative Examples 1 and 3 did not add hindered phenol-based antioxidant flame retardants, and the flame retardancy of polypropylene was the worst.

[0056] Comparative Example 2 did not add the polypropylene grafted glycidyl methacrylate compatibilizer, and had poor compatibility and dispersibility with the polypropylene resin, did not have a good flame retardant effect, and had a limiting oxygen index lower than that of the embodiments.

[0057] The impact strength of polypropylene composite material specimens was tested according to GB / T 1043.1-2008 standard.

[0058] The polypropylene composite material was placed in an accelerated aging test chamber for thermal oxidation aging at a temperature of 80°C for 240 hours; and then the impact strength and tensile strength of the polypropylene composite material specimens were tested.

[0059]

[0060] Each embodiment uses tartaric acid ester hindered phenol, tartaric acid dimethyl phosphate, 1,3-bis (3-aminopropyl) -1,1,3,3-tetramethyl disiloxane for copolymerization to obtain a hindered phenol-based antioxidant flame retardant, whose main chain contains a flexible organosiloxane structure, which has a toughening effect on polypropylene and significantly improves the notched impact strength. In addition, the bis-hindered phenol structure can correct the peroxy radicals, hydroxyl radicals, etc. generated during the thermal oxidative aging of polypropylene, inhibit the thermal oxidative aging reaction process, thereby improving the thermal oxidizability and weather resistance of polypropylene. After accelerated thermal oxidative aging experiments, the notched impact strength of polypropylene decreases very little.

[0061] In Comparative Example 1, no hindered phenol-based antioxidant flame retardant was added, and the thermal oxidation resistance and weather resistance of polypropylene were poor. In the accelerated thermal oxidation aging test, the notched impact strength of polypropylene decreased significantly.

[0062] Comparative Example 2 did not add polypropylene grafted glycidyl methacrylate compatibilizer, hindered phenol-based antioxidant flame retardant, and had poor compatibility and dispersibility with polypropylene resin, did not significantly improve the notched impact strength of polypropylene, and had poor toughening effect.

[0063] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A weather-resistant polypropylene composite material, characterized in that: The invention comprises the following components in parts by weight: 87-98 parts of polypropylene resin, 0.3-2.5 parts of polypropylene grafted glycidyl methacrylate, 1-8 parts of hindered phenol-based antioxidant flame retardant, and 0.5-2 parts of lubricant; The hindered phenol-based antioxidant flame retardant is prepared according to the following method: Add N-methylpyrrolidone, tartrate-based hindered phenol, tartrate-based dimethyl phosphate, and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to a reaction bottle, add pyridine and triphenyl phosphite after stirring, introduce nitrogen, react at a temperature of 100-125° C. for 2-5 hours, and after cooling, pour the solution into a methanol aqueous solution to precipitate, filter, and wash with ethanol to obtain a hindered phenol-based antioxidant flame retardant; The structural formula of the tartrate-based hindered phenol is: The structural formula of tartaric acid dimethyl phosphate is:

2. The weather-resistant polypropylene composite material according to claim 1, characterized in that: The molar ratio of the tartrate hindered phenol, tartrate dimethyl phosphate and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is (0.2-0.5):(0.5-0.8):

1.

3. The weather-resistant polypropylene composite material according to claim 2, characterized in that: The preparation method of the tartrate hindered phenol is as follows: N,N-dimethylformamide, D,L-tartaric acid, 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and triethylamine are added to a reaction bottle, ethyl acetate and water are added after the reaction, extraction and separation are performed, the organic phase is dried, concentrated and recrystallized to obtain the tartrate hindered phenol.

4. The weather-resistant polypropylene composite material according to claim 3, characterized in that: The molar ratio of the D,L-tartaric acid, 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and triethylamine is 1:(2-2.2):(1.8-2.3).

5. The weather-resistant polypropylene composite material according to claim 4, characterized in that: The reaction is first carried out at room temperature for 6-12 hours, and then heated to 55-65° C. for 4-8 hours.

6. The weather-resistant polypropylene composite material according to claim 2, characterized in that: The preparation method of the tartaric acid dimethyl phosphate is as follows: add any solvent of acetone, tetrahydrofuran, ethyl acetate, acetonitrile, D,L-tartaric acid, O,O-dimethylphosphoryl chloride, and triethylamine into a reaction bottle, react, concentrate the solvent, and recrystallize with ethanol to obtain the tartaric acid dimethyl phosphate.

7. The weather-resistant polypropylene composite material according to claim 6, characterized in that: The molar ratio of the D,L-tartaric acid, O,O-dimethylphosphoryl chloride and triethylamine is 1:(2-2.4):(2-2.6).

8. The weather-resistant polypropylene composite material according to claim 6, characterized in that: The reaction is first carried out at 0-10°C for 0.5-1 h, and then the temperature is raised to 25-40°C for 6-18 h.

9. A method for preparing the weather-resistant polypropylene composite material according to any one of claims 1 to 8, characterized in that: 87-98 parts of polypropylene resin, 0.3-2.5 parts of polypropylene grafted glycidyl methacrylate, 1-8 parts of hindered phenol-based antioxidant flame retardant, and 0.5-2 parts of lubricant are added into a twin-screw extruder, the screw speed is 30-80r / min, the melting temperature is 180-190°C, and extrusion granulation is performed to obtain a weather-resistant polypropylene composite material.

10. Use of the weather-resistant polypropylene composite material prepared by the preparation method according to claim 9 in a battery shell of a new energy vehicle.