Linear probe and method for manufacturing the same

By combining capillary correction and vacuum annealing with laser cutting and electrochemical etching technology, the problem of difficulty in straightening and cutting ultra-fine wires in traditional processes is solved, and high-precision and low-cost linear probe production is achieved, which is suitable for small batch production.

CN118191384BActive Publication Date: 2024-10-01SHANGHAI ZENFOCUS SEMI-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211606213.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-10-01
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

It is difficult to effectively straighten and cut wires with a diameter of less than 30 microns using traditional processes, and the cost of traditional equipment is high, making it unsuitable for small batch diversified probe production.

Method used

Using capillary correction combined with vacuum annealing stress relief process, using laser cutting and electrochemical etching technology to prepare linear probes, including threading the ring material into the capillary tube for vacuum annealing, fixing it on the UV protective film for laser cutting, and forming it through electrochemical etching Needle point.

Benefits of technology

It improves the accuracy of wire straightening and cutting errors, reduces production costs, is suitable for small batch diversified probe production, and the process is simple and safe.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118191384B_ABST
    Figure CN118191384B_ABST
Patent Text Reader

Abstract

The present invention provides a linear probe and a manufacturing method thereof, which belongs to the field of probe manufacturing. The method comprises: inserting a probe substrate of a ring material into a capillary tube whose straightness is 0.2% of the length, and placing the probe substrate and the capillary tube together in a vacuum annealing furnace, and heating the probe substrate and the capillary tube until the vacuum degree reaches at least 5*10 ‑3 Pa, vacuum annealing is performed at 350-400°C until the straightness of the probe ring material reaches 0.3% of the material length; the straightened probe substrate is fixed on the UV protective film; the probe substrate on the UV protective film is cut by laser; the cut probe substrate is peeled off from the UV protective film to obtain a probe of a predetermined length; the probe is micro-etched and deoxidized to obtain a preliminary finished product; one end of the preliminary finished product is sharpened by electrochemical etching to obtain a linear probe. The processing scheme disclosed in the present invention improves the accuracy of the cutting error.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of probe manufacturing, and in particular to a linear probe and a manufacturing method thereof. Background Art

[0002] Usually, for wires with a diameter of less than 30 microns, material suppliers can only provide coils, that is, the materials are rolled after the drawing process. In order to be processed into linear probes that meet the use conditions, the coils must be straightened and cut. For wires with a wire diameter below 30um, it is difficult to correct them using traditional correction processes. On the one hand, the wire diameter is too small to withstand a limited force, and the material itself has a low elongation. The use of traction and stretching correction has a high material breakage rate during the correction process; on the other hand, the material hardness is low, and it is easy to scratch the surface of the coil when passing through the correction guide mechanism, and the scratched part will become a defect in subsequent use. Not only that, the traditional process is difficult to control the error in needle length, which is usually around 30 microns, and cannot meet the current required 10 micron cutting error; and the traditional machine cutting section is shear-shaped, has burrs, and the section flatness is very poor. At present, relevant manufacturers can provide complete straightening and cutting equipment, but the equipment is expensive, and the mold needs to be replaced for wires with different wire diameters, which greatly increases the production cost and is completely unsuitable for small-batch diversified probe production.

[0003] In addition, the traditional method for making the needle tip on a wire needle of about 30um is mechanical grinding. This method involves a probe automatic loading module, a probe fixing module, and a probe rotating grinding module. These devices are relatively expensive and are also not suitable for small batch diversified probe production. Summary of the invention

[0004] Therefore, in order to overcome the above-mentioned shortcomings of the prior art, the present invention provides a linear probe and a method for manufacturing the same.

[0005] In order to achieve the above object, the present invention provides a method for manufacturing a linear probe, comprising: inserting a 5-probe substrate of a ring material into a capillary tube with a straightness of 0.2% of the length, and placing the probe substrate and the capillary tube together in a vacuum annealing furnace, and annealing the probe substrate in a vacuum furnace at least 5*10 -3 Pa, vacuum annealing is performed at 350-400°C until the straightness of the probe coil reaches 0.3% of the material length; the straightened probe substrate is fixed on the UV protective film; the probe substrate on the UV protective film is cut by laser; the cut

[0006] The probe substrate is peeled off from the UV protective film to obtain a probe of a predetermined length; the probe is subjected to micro-etching to remove oxidation to obtain a preliminary finished product; and one end of the preliminary finished product is sharpened by electrochemical etching to obtain a linear probe.

[0007] In one embodiment, the difference between the inner diameter of the capillary and the outer diameter of the probe substrate is in the range of 10 to 25 μm.

[0008] In one embodiment, the probe substrate and the capillary are placed in a vacuum annealing furnace and the vacuum reaches at least 5*10 -3 Vacuum annealing at 350-400°C for 1.5-2 hours under the condition of Pa.

[0009] In one embodiment, the thickness of the UV protection film is not less than 100 μm.

[0010] In one embodiment, the parameters of laser cutting are: laser wavelength 350-370nm, laser pulse width less than 350um, laser frequency 600-650KHz, power 3-5W, scanning speed 400-500mm / s.

[0011] In one embodiment, the micro-etching and deoxidation treatment of the probe to obtain a preliminary finished product includes: immersing the probe in an ultrasonic bath of 2-5% dilute sulfuric acid for 30 seconds to obtain a preliminary finished product.

[0012] In one embodiment, the use of electrochemical etching to sharpen one end of the primary product to obtain a linear probe comprises: 3 PO 4 and ethanol in a volume ratio of 7:3 to prepare an electrolytic solution; the pre-finished product is used as an anode and the platinum-iridium alloy is used as a cathode. When the anode electromotive force is not less than 2V, electrochemical corrosion occurs at the position where the pre-finished product contacts the electrolyte, and a needle tip is formed to obtain a linear probe.

[0013] A linear probe, characterized in that the linear probe is prepared by the above method.

[0014] Compared with the prior art, the advantages of the present invention are: the use of capillary correction combined with vacuum annealing to relieve stress solves the problem that the traditional process cannot straighten ultra-fine wires, and then the laser can be used to process the probe ring material, which has fewer processes and improves the accuracy of cutting errors. In addition, the use of electrochemical corrosion to sharpen the cross section of the linear probe material not only solves the problem that the traditional process cannot sharpen wires with a wire diameter of less than 30 microns, but also has simple and safe manual operation, easy and cheap raw materials and equipment, and high preparation efficiency and success rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0016] Figure 1 is a flow chart of a method for manufacturing a linear probe in an embodiment of the present invention;

[0017] Figure 2 Schematic diagram of electrochemical corrosion in an embodiment of the present invention. DETAILED DESCRIPTION

[0018] The embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.

[0019] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present disclosure, rather than all of the embodiments. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present disclosure. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present disclosure.

[0020] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present disclosure, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number of aspects described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0021] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present disclosure. The drawings only show components related to the present disclosure rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0022] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0023] like Figure 1 As shown, the present disclosure provides a method for manufacturing a linear probe, comprising:

[0024] Step 101: insert the probe substrate of the coil into a capillary tube with a straightness of 0.2% of the length, and put the probe substrate and the capillary tube into a vacuum annealing furnace. -3 Vacuum annealing is performed at 350-400°C under the condition of Pa until the straightness of the probe ring material reaches 0.3% of the material length.

[0025] Insert the probe substrate of the coil into a capillary tube with a straightness of 0.2% of its length, and put the probe substrate and the capillary tube into a vacuum annealing furnace. -3 Vacuum annealing is performed at 350-400°C under the condition of 200 Pa until the straightness of the probe coil reaches 0.3% of the material length. In one embodiment, the difference between the inner diameter of the capillary and the outer diameter of the probe substrate is in the range of 10 to 25 μm. Taking Φ30um AgCu wire as an example, the requirements for the capillary can be 50 μm inner diameter, 365 μm outer diameter, 300 mm length, and a straightness of 0.2% of the length. The straightness of the capillary changes little at high temperature. The capillary can be 15-30 cm, preferably 15 to 20 cm.

[0026] Put the wire and capillary to be straightened into a vacuum annealing furnace and anneal them at 350-400℃ for 1.5-2 hours to ensure that the surface stress of the wire is completely removed and the straightness reaches 0.3% of the material length. The vacuum degree should be at least 5*10 -3 The pa condition can ensure that the material does not oxidize during heat treatment. The annealing temperature of 350-400℃ is to avoid recrystallization of AgCu materials when the temperature is too high and to prevent the decrease in material strength caused by grain growth. 1-1.5h is to reduce the high cost of heat treatment.

[0027] Step 102, fixing the straightened probe substrate on a UV protective film.

[0028] Since the probe substrate has a small wire diameter, it is very easy to deform during cutting. Fixing the material on the UV protective film can ensure that the probe substrate has a certain rigidity during processing and reduce deformation. In one embodiment, the thickness of the UV protective film is not less than 100μm. The film thickness determines the overall rigidity of the product during cutting. If the film thickness is small, the overall rigidity is poor, and the probe is easy to deform during cutting. There is a layer of glue on the UV film, and the material and the film can be connected together through the glue.

[0029] Step 103 , using a laser to cut the probe substrate on the UV protective film.

[0030] In this step, femtosecond, picosecond or other cold laser cutting can be used. By using ultrashort laser to cut the probe substrate, linear probe processing can be performed quickly without affecting the mechanical properties of the probe alloy material. In one embodiment, the parameters of laser cutting are: laser wavelength 350-370nm, laser pulse width less than 350um, laser frequency 600-650KHz, power 3-5W, scanning speed 400-500mm / s.

[0031] Step 104 , peeling the cut probe substrate from the UV protective film to obtain a probe of a predetermined length.

[0032] The UV protective film mentioned in step 102 is irradiated with an LED light having a main wavelength of 350-380 nm. The glue on the UV film is invalidated by irradiation, so that the probe that has been cut can be easily peeled off from the film.

[0033] Step 105, performing micro-etching and deoxidation treatment on the probe to obtain a preliminary finished product.

[0034] The probe can be micro-etched and deoxidized in a slightly acidic environment to obtain a preliminary finished product. In one embodiment, the probe is immersed in an ultrasonic bath with a mass fraction of 2-5% dilute sulfuric acid for 30-45 seconds to obtain a preliminary finished product.

[0035] Step 106, using electrochemical etching to sharpen one end of the preliminary finished product to obtain a linear probe.

[0036] like Figure 2 As shown, electrochemical corrosion is used to sharpen one end of the pre-finished product to obtain a linear probe. The pre-finished product is used as the anode and the platinum-iridium alloy is used as the cathode. When the anode electromotive force is not less than 2V, electrochemical corrosion occurs at the position where the pre-finished product contacts the electrolyte, and a needle tip is formed to obtain a linear probe. During electrochemical corrosion, the voltage remains unchanged, and the current will continue to decrease. When the current is zero, the corrosion ends. At this time, the pre-finished product breaks at the liquid surface and breaks into two pieces, each end of which is a formed needle tip.

[0037] In one embodiment, a medium strength inorganic tribasic acid H 3 PO4 and ethanol in a volume ratio of 7:3 to form an electrolytic solution; the pre-finished product is used as the anode and the platinum-iridium alloy is used as the cathode. When the anode electromotive force is not less than 2V, electrochemical corrosion occurs at the contact position between the pre-finished product and the electrolyte, and a needle tip is formed to obtain a linear probe. 3 PO 4 It can be H with a mass fraction of 40-60% 3 PO 4 .

[0038] A linear probe is prepared by adopting the above method.

[0039] The above method uses the process of capillary correction combined with vacuum annealing to relieve stress to solve the problem that traditional processes cannot straighten ultra-fine wires, and then the probe ring material can be processed by laser, which has fewer processes and improves the accuracy of cutting errors. In addition, the use of electrochemical corrosion to sharpen the cross section of the linear probe material not only solves the problem that traditional processes cannot sharpen wires with a wire diameter of less than 30 microns, but also makes manual operation simple and safe, raw materials and equipment are easy to obtain and cheap, and the preparation efficiency and success rate are high.

[0040] The above is only a specific implementation of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A method for manufacturing a linear probe, characterized in that: include: The probe substrate of the coil is inserted into a capillary tube with a straightness of 0.2% of the length, and the probe substrate and the capillary tube are placed in a vacuum annealing furnace. -3 Vacuum annealing is performed at 350-400° C. under the condition of 1.5 Pa until the straightness of the probe coil reaches 0.3% of the material length, the probe substrate is a wire with a diameter of less than 30 μm, and the coil is a material rolled after a drawing process; Fixing the straightened probe substrate on the UV protective film; Use laser to cut the probe substrate on the UV protective film; Peeling the cut probe substrate off the UV protective film to obtain a probe of a predetermined length; Performing micro-etching and deoxidation treatment on the probe to obtain a preliminary finished product; One end of the preformed product was sharpened using electrochemical etching to obtain a linear probe.

2. The method according to claim 1, characterized in that The difference between the inner diameter of the capillary and the outer diameter of the probe substrate is in the range of 10 to 25 μm.

3. The method according to claim 1, characterized in that The probe substrate and the capillary are placed in a vacuum annealing furnace and the vacuum degree reaches at least 5*10 -3 Vacuum annealing at 350-400°C for 1.5-2 hours under the condition of Pa.

4. The method according to claim 1, characterized in that: The thickness of the UV protective film is not less than 100 μm.

5. The method according to claim 1, characterized in that The parameters of laser cutting are: laser wavelength 350-370nm, laser pulse width less than 350um, laser frequency 600-650KHz, power 3-5W, scanning speed 400-500mm / s.

6. The method according to claim 1, characterized in that The step of performing micro-etching and deoxidation treatment on the probe to obtain a preliminary finished product comprises: The probe is immersed in an ultrasonic bath containing 2-5% by mass percent dilute sulfuric acid for 30-45 seconds for cleaning to obtain a primary finished product.

7. The method according to claim 1, characterized in that The method of using electrochemical corrosion to sharpen one end of the pre-finished product to obtain a linear probe comprises: The medium-strength inorganic tribasic acid H3PO4 and ethanol are mixed in a volume ratio of 7:3 to prepare an electrolytic solution; The preliminary product is used as an anode and the platinum-iridium alloy is used as a cathode. When the anode electromotive force is not less than 2V, electrochemical corrosion occurs at the position where the preliminary product contacts the electrolyte, and a needle tip is formed to obtain a linear probe.

8. A linear probe, characterized in that: The linear probe is prepared by the method according to any one of claims 1 to 7.