High-strength plastic for automobile interior parts and preparation method thereof
By using a combination of PBT, glass fiber, homemade chain extender and ionic polymer in automotive interior parts, the problems of poor heat resistance and low strength of existing PBT plastics are solved, and the heat of automotive interior parts is significantly improved. Stability and strength.
Patent Information
- Application Number
- CN202410401433.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-04-03
AI Technical Summary
Existing PBT plastics have poor heat resistance and low strength in automotive interior parts, which cannot meet the high performance needs of automotive interior parts.
High-strength plastics including PBT, glass fiber, homemade chain extenders and ionic polymers, homemade chain extenders produced by reactions of cyclohexylbenzide, diphenyl phosphate chloride and neopentyl glycol, and vinyl The ionic polymer produced by reacting ethylene glycol imidazole homopolymer with carboxy hyperbranched polyester enhances the thermal stability and strength of the plastic.
It significantly improves the thermal stability and strength of plastics for automotive interior parts, meeting the needs of high-performance automotive interior parts.
Smart Images

Figure BDA0004775766660000091 
Figure BDA0004775766660000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastics, in particular to a high-strength plastic for automobile interior decoration parts and a preparation method thereof. Background Art
[0002] Automotive interior parts mainly refer to automotive products used for interior modification of automobiles, involving all aspects of the interior of the automobile, such as glove boxes, car seat backs, car inlays, car side panels, pillar guards, door panels, car sub-instrument panels, glove boxes, radio boxes and central consoles, etc. are all automotive interior parts. The automotive interior system is an important part of the car body, and the design workload of the interior system accounts for more than 60% of the workload of the car styling design, far exceeding the car's appearance, and is one of the most important parts of the car body.
[0003] PBT is formed by the polycondensation of 1,4-butanediol and terephthalic acid or terephthalate, and has very good chemical stability, mechanical strength, electrical insulation properties and thermal stability, and is widely used in household appliances, electrical components and the automotive industry. However, the PBT plastics currently used generally have the disadvantages of poor heat resistance and low strength. Therefore, the present invention studies and prepares a high-strength plastic for high-toughness automotive interior parts to solve this problem. Summary of the invention
[0004] The object of the present invention is to provide a high-strength plastic for automobile interior decoration parts and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a high-strength plastic for automobile interior decoration parts, wherein the high-strength plastic for automobile interior decoration parts comprises PBT, glass fiber, a homemade chain extender, an ionic polymer and an antioxidant 1010.
[0006] Preferably, the homemade chain extender is prepared by reacting cyclohexylbenzamide, diphenyl chlorinated phosphate and neopentyl glycol.
[0007] Preferably, the cyclohexylbenzamide is prepared by first reacting trimesic acid with triphosgene and then reacting with cyclohexylamine for amidation.
[0008] Preferably, the ionic polymer is obtained by reacting a vinyl glycol imidazole homopolymer with a carboxyl hyperbranched polyester; the vinyl glycol imidazole homopolymer is obtained by reacting N-vinyl imidazole with bromoacetaldehyde glycol acetal and then polymerizing the monomers.
[0009] Preferably, a method for preparing a high-strength plastic for automotive interior parts comprises the following specific steps:
[0010] (1) Cyclohexylamine and ethyl acetate are mixed at a mass ratio of 2.3 to 2.5:1, stirred in an ice bath, and then cyclohexylbenzamide matrix (3.2 to 3.4 times the mass of cyclohexylamine) is added dropwise at a rate of 1 to 3 mL / min, the temperature is raised to 60 to 70° C., refluxed for 7 to 9 hours, filtered and washed with sodium hydroxide solution for 3 to 5 times, filtered and then washed with deionized water for 3 to 5 times, and finally filtered and dried to obtain cyclohexylbenzamide;
[0011] (2) diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide were mixed, reacted in an ice bath for 4 to 6 hours, heated to 70 to 90° C., refluxed for 50 to 70 minutes, rotary evaporated, washed with water, 5% sodium carbonate solution and water for 3 to 5 times, and dried to obtain a homemade chain extender;
[0012] (3) mixing ethylene glycol imidazole, methanol and azobisisobutyronitrile in a mass ratio of 1 to 2:40:0.02, heating in a water bath to 68 to 72° C., reacting for 24 to 28 hours, drying, purifying with methanol, and drying again to obtain ethylene glycol imidazole homopolymer;
[0013] (4) mixing the terminal hydroxyl hyperbranched polyester with acetone in a mass ratio of 1 to 3:50, adding succinic anhydride of equal mass to the terminal hydroxyl hyperbranched polyester and catalyst triethylamine of 0.35 to 0.45 times the mass of the terminal hydroxyl hyperbranched polyester, heating to 58 to 62° C., reacting for 4 to 6 hours, precipitating with ethanolic sodium hydroxide solution and filtering, then washing with anhydrous ethanol for 3 to 5 times, and finally drying in vacuum at 50° C. to obtain a carboxyl hyperbranched polyester;
[0014] (5) mixing a carboxyl hyperbranched polyester and a vinyl glycol imidazole homopolymer in a mass ratio of 3 to 5:1, heating to 90 to 120° C., and adding concentrated sulfuric acid in an amount of 0.03 to 0.06 times the mass of the carboxyl hyperbranched polyester dropwise at a rate of 1 to 3 mL / min to obtain an ionic polymer;
[0015] (6) PBT and glass fiber are dried at 60-70° C., the dried PBT, dried glass fiber, homemade chain extender, ionic polymer and antioxidant 1010 are mixed in a mass ratio of 30:1-4:0.3-0.5:0.06:0.04, and extruded through a twin-screw extruder to obtain a high-strength plastic for automotive interior parts.
[0016] Preferably, in the above step (1): the preparation method of the cyclohexylbenzamide matrix is: trimesic acid, triphosgene and ethyl acetate are mixed in a mass ratio of 3.1 to 3.3:12:13, heated to 25 to 28° C. in a water bath, 0.45 to 0.55 times the mass of trimesic acid as initiator N,N-dimethylformamide is added, and 0.8 to 0.9 times the mass of trimesic acid as ethyl acetate is added dropwise at a rate of 1 to 3 mL / min, the temperature is continued to be raised to 60 to 65° C., and the reaction is carried out for 7 to 8 hours to obtain the cyclohexylbenzamide matrix.
[0017] Preferably, in the above step (2), the mass ratio of diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide is 10:1.5:3:1:4:5-7.
[0018] Preferably, in the above step (3): the preparation method of vinyl glycol imidazole is: N-vinyl imidazole, bromoacetaldehyde ethylene glycol acetal and methanol are mixed in a mass ratio of 8-10:9:120, heated to 36-40°C in a water bath, stirred and reacted at 80-100 rpm for 20-40 min, heated to 52-56°C, continued to react for 4-6 h, cooled to room temperature and washed with ethyl acetate for 3-5 times, and rotary evaporated to obtain vinyl glycol imidazole.
[0019] Preferably, in the above step (4): the preparation method of the terminal hydroxyl hyperbranched polyester is: under a nitrogen atmosphere, trimethylolpropane, 2,2-dimethylolpropionic acid and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 1.1-1.3:9:0.1, the temperature is raised to 135-145°C, and after reacting for 2-4 hours, the temperature is sealed and evacuated, and the temperature is further reacted for 2-4 hours, and after the temperature is lowered to 40-50°C, it is dissolved with acetone and precipitated with n-hexane, and finally dried at 50-60°C to obtain the terminal hydroxyl hyperbranched polyester.
[0020] Preferably, in the above step (6): the extrusion temperature of the extruder is 240-260°C.
[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0022] The high-strength plastic for automobile interior decoration parts prepared by the present invention comprises PBT, glass fiber, a homemade chain extender and an ionic polymer;
[0023] The homemade chain extender is prepared by the reaction of cyclohexylbenzamide, diphenyl phosphate chloride and neopentyl glycol. Cyclohexylbenzamide is prepared by first reacting trimesic acid with triphosgene and then reacting with cyclohexylamine for amidation. The three amide bonds in cyclohexylbenzamide can react with neopentyl glycol, and diphenyl phosphate chloride is introduced at the same time, so that the homemade chain extender has cyclohexyl and diphenyl phosphate, which can jointly extend the chain of plastics and synergistically improve the thermal stability of plastics.
[0024] The ionic polymer is prepared by the reaction of vinyl glycol imidazole homopolymer and carboxyl hyperbranched polyester. The vinyl glycol imidazole homopolymer is prepared by the reaction of N-vinyl imidazole and bromoacetaldehyde glycol acetal followed by monomer polymerization, and then reacted with carboxyl hyperbranched polyester to form an ionic polymer with a dendritic structure and imidazole as the center. The carboxyl group in the ionic polymer can react with the amino group on the glass fiber to form an ionomer, and undergo an ion exchange reaction with the terminal carboxyl group of PBT to form an end group product with ions, thereby enhancing the compatibility of PBT with the glass fiber, thereby enhancing the strength of the plastic. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high-strength plastics for automotive interior trims prepared in the examples and comparative examples as follows:
[0027] Heat resistance: The automotive interior parts prepared in the examples and comparative examples were subjected to heat deformation temperature and humidity tests using high-strength plastics according to ISO-75-1.
[0028] Tensile strength: The automotive interior trim parts prepared in the examples and comparative examples were subjected to a tensile strength test using high-strength plastics according to GB / T1447.
[0029] Example 1
[0030] (1) Trimesic acid, triphosgene and ethyl acetate are mixed in a mass ratio of 3.1:12:13, heated to 25°C in a water bath, an initiator N,N-dimethylformamide is added in an amount of 0.45 times the mass of trimesic acid, and ethyl acetate is added dropwise at a rate of 1 mL / min in an amount of 0.8 times the mass of trimesic acid, and the temperature is continued to be raised to 60°C, and the reaction is carried out for 7 hours to obtain a cyclohexylbenzamide matrix; cyclohexylamine and ethyl acetate are mixed in a mass ratio of 2.3:1, stirred in an ice bath, and cyclohexylbenzamide matrix is added dropwise at a rate of 1 mL / min in an amount of 3.2 times the mass of cyclohexylamine, and the temperature is raised to 60°C, refluxed for 7 hours, filtered and washed with sodium hydroxide solution for 3 times, filtered and washed with deionized water for 3 times, and finally filtered and dried to obtain cyclohexylbenzamide;
[0031] (2) Diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide were mixed in a mass ratio of 10:1.5:3:1:4:5, reacted in an ice bath for 4 hours, heated to 70°C, refluxed for 50 minutes, rotary evaporated and washed three times with water, 5% sodium carbonate solution and water, and dried to obtain a homemade chain extender;
[0032] (3) N-vinyl imidazole, bromoacetaldehyde glycol acetal and methanol were mixed in a mass ratio of 8:9:120, heated to 36°C in a water bath, stirred at 80 rpm for 20 min, heated to 52°C, continued to react for 4 h, cooled to room temperature and washed with ethyl acetate three times, and rotary evaporated to obtain vinyl glycol imidazole; vinyl glycol imidazole, methanol and azobisisobutyronitrile were mixed in a mass ratio of 1:40:0.02, heated to 68°C in a water bath, reacted for 24 h, dried, purified with methanol, and dried again to obtain vinyl glycol imidazole homopolymer;
[0033] (4) In a nitrogen atmosphere, trimethylolpropane, 2,2-dimethylolpropionic acid and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 1.1:9:0.1, heated to 135°C, reacted for 2 hours, sealed and evacuated, and reacted for another 2 hours. After the temperature is lowered to 40°C, the mixture is dissolved in acetone, precipitated with n-hexane, and finally dried at 50°C to obtain a terminal hydroxyl hyperbranched polyester; the terminal hydroxyl hyperbranched polyester is mixed with acetone in a mass ratio of 1:50, succinic anhydride of the same mass as the terminal hydroxyl hyperbranched polyester and catalyst triethylamine of 0.35 times the mass of the terminal hydroxyl hyperbranched polyester are added, the temperature is raised to 58°C, reacted for 4 hours, precipitated with an ethanolic sodium hydroxide solution and filtered, then washed with anhydrous ethanol for 3 times, and finally dried in a vacuum at 50°C to obtain a carboxyl hyperbranched polyester;
[0034] (5) mixing a carboxyl hyperbranched polyester and a vinyl glycol imidazole homopolymer in a mass ratio of 3:1, heating to 90° C., and adding concentrated sulfuric acid in an amount of 0.03 times the mass of the carboxyl hyperbranched polyester dropwise at a rate of 1 mL / min to prepare an ionic polymer;
[0035] (6) PBT and glass fiber were dried at 60° C., the dried PBT, dried glass fiber, homemade chain extender, ionic polymer and antioxidant 1010 were mixed in a mass ratio of 30:1:0.3:0.06:0.04, and extruded through a twin-screw extruder at an extrusion temperature of 240° C. to obtain a high-strength plastic for automotive interior parts.
[0036] Example 2
[0037] (1) Trimesic acid, triphosgene and ethyl acetate are mixed in a mass ratio of 3.2:12:13, heated to 26°C in a water bath, an initiator N,N-dimethylformamide in an amount of 0.45 to 0.55 times the mass of trimesic acid is added, and ethyl acetate in an amount of 0.85 times the mass of trimesic acid is added dropwise at a rate of 2 mL / min, the temperature is continued to be raised to 63°C, and the reaction is carried out for 7.5 hours to obtain a cyclohexylbenzamide matrix; cyclohexylamine and ethyl acetate are mixed in a mass ratio of 2.4:1, stirred in an ice bath, and cyclohexylbenzamide matrix in an amount of 3.3 times the mass of cyclohexylamine is added dropwise at a rate of 2 mL / min, the temperature is raised to 65°C, refluxed for 8 hours, filtered and washed with sodium hydroxide solution 4 times, filtered and washed with deionized water 4 times, and finally filtered and dried to obtain cyclohexylbenzamide;
[0038] (2) Diphenyl chlorophosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide were mixed in a mass ratio of 10:1.5:3:1:4:6, reacted in an ice bath for 5 h, heated to 80° C., refluxed for 60 min, rotary evaporated and washed four times with water, 5% sodium carbonate solution and water, and dried to obtain a homemade chain extender;
[0039] (3) N-vinyl imidazole, bromoacetaldehyde glycol acetal and methanol were mixed in a mass ratio of 9:9:120, heated to 38°C in a water bath, stirred at 90 rpm for 30 min, heated to 54°C, continued to react for 5 h, cooled to room temperature and washed with ethyl acetate 4 times, and rotary evaporated to obtain vinyl glycol imidazole; vinyl glycol imidazole, methanol and azobisisobutyronitrile were mixed in a mass ratio of 1.5:40:0.02, heated to 70°C in a water bath, reacted for 26 h, dried, purified with methanol, and dried again to obtain vinyl glycol imidazole homopolymer;
[0040] (4) In a nitrogen atmosphere, trimethylolpropane, 2,2-dimethylolpropionic acid and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 1.2:9:0.1, heated to 140°C, reacted for 3 hours, sealed and evacuated, and reacted for 3 hours. After cooling to 45°C, the mixture is dissolved in acetone, precipitated with n-hexane, and finally dried at 55°C to obtain a terminal hydroxyl hyperbranched polyester; the terminal hydroxyl hyperbranched polyester is mixed with acetone in a mass ratio of 2:50, succinic anhydride of the same mass as the terminal hydroxyl hyperbranched polyester and catalyst triethylamine of 0.4 times the mass of the terminal hydroxyl hyperbranched polyester are added, heated to 50°C, reacted for 5 hours, precipitated with ethanolic sodium hydroxide solution and filtered, then washed with anhydrous ethanol 4 times, and finally dried in vacuum at 50°C to obtain a carboxyl hyperbranched polyester;
[0041] (5) mixing a carboxyl hyperbranched polyester and a vinyl glycol imidazole homopolymer in a mass ratio of 4:1, heating to 110° C., and adding concentrated sulfuric acid in an amount of 0.045 times the mass of the carboxyl hyperbranched polyester dropwise at a rate of 2 mL / min to obtain an ionic polymer;
[0042] (6) PBT and glass fiber were dried at 65° C., the dried PBT, dried glass fiber, homemade chain extender, ionic polymer and antioxidant 1010 were mixed in a mass ratio of 30:3:0.4:0.06:0.04, and extruded through a twin-screw extruder at an extrusion temperature of 250° C. to obtain a high-strength plastic for automotive interior parts.
[0043] Example 3
[0044] (1) Trimesic acid, triphosgene and ethyl acetate are mixed in a mass ratio of 3.3:12:13, heated to 28° C. in a water bath, an initiator N,N-dimethylformamide is added in an amount of 0.55 times the mass of trimesic acid, and ethyl acetate is added dropwise at a rate of 3 mL / min in an amount of 0.9 times the mass of trimesic acid, and the temperature is continued to be raised to 65° C., and the reaction is carried out for 8 hours to obtain a cyclohexylbenzamide matrix; cyclohexylamine and ethyl acetate are mixed in a mass ratio of 2.5:1, stirred in an ice bath, and cyclohexylbenzamide matrix is added dropwise at a rate of 3 mL / min in an amount of 3.4 times the mass of cyclohexylamine, and the temperature is raised to 70° C., refluxed for 9 hours, filtered and washed with sodium hydroxide solution 5 times, filtered and washed with deionized water 5 times, and finally filtered and dried to obtain cyclohexylbenzamide;
[0045] (2) diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide were mixed in a mass ratio of 10:1.5:3:1:4:7, reacted in an ice bath for 6 hours, heated to 90°C, refluxed for 70 minutes, rotary evaporated and washed with water, 5% sodium carbonate solution and water for 5 times, and dried to obtain a homemade chain extender;
[0046] (3) N-vinyl imidazole, bromoacetaldehyde glycol acetal and methanol were mixed in a mass ratio of 10:9:120, heated to 40°C in a water bath, stirred at 100 rpm for 40 min, heated to 56°C, continued to react for 6 h, cooled to room temperature and washed with ethyl acetate 5 times, and rotary evaporated to obtain vinyl glycol imidazole; vinyl glycol imidazole, methanol and azobisisobutyronitrile were mixed in a mass ratio of 2:40:0.02, heated to 72°C in a water bath, reacted for 28 h, dried, purified with methanol, and dried again to obtain vinyl glycol imidazole homopolymer;
[0047] (4) In a nitrogen atmosphere, trimethylolpropane, 2,2-dimethylolpropionic acid and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 1.3:9:0.1, heated to 145°C, reacted for 4 hours, sealed and evacuated, and reacted for another 4 hours. After the temperature was lowered to 50°C, the mixture was dissolved in acetone, precipitated with n-hexane, and finally dried at 60°C to obtain a terminal hydroxyl hyperbranched polyester; the terminal hydroxyl hyperbranched polyester and acetone were mixed in a mass ratio of 3:50, succinic anhydride of the same mass as the terminal hydroxyl hyperbranched polyester and catalyst triethylamine of 0.45 times the mass of the terminal hydroxyl hyperbranched polyester were added, the temperature was raised to 62°C, reacted for 6 hours, precipitated with an ethanolic sodium hydroxide solution and filtered, then washed with anhydrous ethanol 5 times, and finally dried in vacuum at 50°C to obtain a carboxyl hyperbranched polyester;
[0048] (5) mixing a carboxyl hyperbranched polyester and a vinyl glycol imidazole homopolymer in a mass ratio of 5:1, heating to 120° C., and adding concentrated sulfuric acid in an amount of 0.06 times the mass of the carboxyl hyperbranched polyester dropwise at a rate of 3 mL / min to obtain an ionic polymer;
[0049] (6) PBT and glass fiber were dried at 70° C., the dried PBT, dried glass fiber, homemade chain extender, ionic polymer and antioxidant 1010 were mixed in a mass ratio of 30:4:0.5:0.06:0.04, and extruded through a twin-screw extruder at an extrusion temperature of 260° C. to obtain a high-strength plastic for automotive interior parts.
[0050] Comparative Example 1
[0051] The prescription composition of comparative example 1 is the same as that of example 2. The difference between the method for preparing the high-strength plastic for automobile interior decoration parts and example 2 is that the homemade chain extender is only cyclohexylbenzamide.
[0052] Comparative Example 2
[0053] The prescription composition of comparative example 2 is the same as that of example 2. The difference between the method for making high-strength plastic for automobile interior decoration parts and example 2 is that the homemade chain extender is only diphenyl chlorinated phosphate.
[0054] Comparative Example 3
[0055] The prescription composition of Comparative Example 3 is the same as that of Example 2. The difference between the method for making the high-strength plastic for automobile interior parts and Example 2 is that the high-strength plastic for automobile interior parts includes PBT, glass fiber and ionomer.
[0056] Comparative Example 4
[0057] The formulation composition of Comparative Example 4 is the same as that of Example 2. The difference between the method for making high-strength plastic for automobile interior parts and Example 2 is that the ionic polymer is only ethylene glycol imidazole homopolymer.
[0058] Comparative Example 5
[0059] The formulation composition of Comparative Example 5 is the same as that of Example 2. The difference between the method for preparing the high-strength plastic for automobile interior parts and Example 2 is that the high-strength plastic for automobile interior parts includes PBT, glass fiber and a homemade chain extender.
[0060] Effect example
[0061] Table 1 below shows the performance analysis results of high-strength plastics for automotive interior trim parts using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5:
[0062] Table 1
[0063]
[0064]
[0065] By comparing the experimental data of the examples and the comparative examples in Table 1, it can be clearly found that the high-strength plastics for automotive interior decoration parts prepared in Examples 1, 2 and 3 have excellent thermal stability and good strength.
[0066] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 3, it can be found that trimesic acid is first reacted with triphosgene, and then with cyclohexylamine to obtain cyclohexylbenzamide through amidation reaction, and then reacted with diphenyl chlorinated phosphate and neopentyl glycol to obtain a homemade chain extender, and diphenyl chlorinated phosphate is introduced at the same time, so that the homemade chain extender has cyclohexyl and diphenyl phosphate, which jointly extend the chain of the plastic and synergistically improve the thermal stability of the plastic;
[0067] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 4 and Comparative Example 5, it can be found that the ionic polymer obtained by reacting N-vinyl imidazole with bromoacetaldehyde glycol acetal and then polymerizing the vinyl glycol imidazole homopolymer and the carboxyl hyperbranched polyester to form an ionic polymer with a dendritic structure and imidazole as the center, and the carboxyl group in the ionic polymer can react with the amino group on the glass fiber to form an ionomer, and undergo an ion exchange reaction with the terminal carboxyl group of PBT to form an ion-carboxyl terminal product, thereby enhancing the compatibility of PBT with the glass fiber, thereby enhancing the strength of the plastic.
[0068] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high-strength plastic for automotive interior parts, It is characterized in that The high-strength plastic for automobile interior parts comprises PBT, glass fiber, a self-made chain extender, an ionic polymer and an antioxidant 1010; the self-made chain extender is prepared by mixing cyclohexylamine and ethyl acetate in a mass ratio of 2.3 to 2.5:1, stirring evenly in an ice bath, adding a cyclohexylbenzamide matrix of 3.2 to 3.4 times the mass of cyclohexylamine at a rate of 1 to 3 mL / min, heating to 60 to 70° C., reflux reaction for 7 to 9 hours, filtering and washing with a sodium hydroxide solution for 3 to 5 minutes. The mixture was filtered and then washed with deionized water for 3 to 5 times, and finally filtered and dried to obtain cyclohexylbenzamide; diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide were mixed, reacted in an ice bath for 4 to 6 hours, heated to 70 to 90°C, refluxed for 50 to 70 minutes, rotary evaporated and washed with water, 5% sodium carbonate solution and water for 3 to 5 times in sequence, and dried to obtain a self-made chain extender; the ionic polymer is Ethylene glycol imidazole, methanol and azobisisobutyronitrile are mixed in a mass ratio of 1-2:40:0.02, heated to 68-72°C in a water bath, reacted for 24-28 hours, dried, purified with methanol, and dried again to obtain ethylene glycol imidazole homopolymer; terminal hydroxyl hyperbranched polyester and acetone are mixed in a mass ratio of 1-3:50, and succinic anhydride of the same mass as the terminal hydroxyl hyperbranched polyester and catalyst triethylamine of 0.35-0.45 times the mass of the terminal hydroxyl hyperbranched polyester are added. The temperature is raised to 58-62°C, reacted for 4-6 hours, precipitated with ethanolic sodium hydroxide solution and filtered, then washed with anhydrous ethanol for 3-5 times, and finally dried in vacuum at 50°C to obtain a carboxyl hyperbranched polyester; the carboxyl hyperbranched polyester and vinyl glycol imidazole homopolymer are mixed in a mass ratio of 3-5:1, the temperature is raised to 90-120°C, and concentrated sulfuric acid in an amount of 0.03-0.06 times the mass of the carboxyl hyperbranched polyester is added dropwise at a rate of 1-3 mL / min to obtain an ionic polymer.
2. A method for preparing high-strength plastic for automotive interior parts, It is characterized in that The method for preparing the high-strength plastic for automobile interior decoration parts comprises the following specific steps: (1) Cyclohexylamine and ethyl acetate are mixed in a mass ratio of 2.3-2.5:1, stirred evenly in an ice bath, and then cyclohexylbenzamide matrix (3.2-3.4 times the mass of cyclohexylamine) is added dropwise at a rate of 1-3 mL / min, the temperature is raised to 60-70°C, refluxed for 7-9 hours, filtered and washed with sodium hydroxide solution for 3-5 times, filtered and then washed with deionized water for 3-5 times, and finally filtered and dried to obtain cyclohexylbenzamide; (2) Diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide were mixed, reacted in an ice bath for 4-6 hours, then heated to 70-90°C, refluxed for 50-70 minutes, rotary evaporated, washed with water, 5% sodium carbonate solution and water for 3-5 times, and dried to obtain a homemade chain extender; (3) Mixing ethylene glycol imidazole, methanol and azobisisobutyronitrile in a mass ratio of 1-2:40:0.02, heating in a water bath to 68-72°C, reacting for 24-28 hours, drying, purifying with methanol, and drying again to obtain ethylene glycol imidazole homopolymer; (4) mixing the terminal hydroxyl hyperbranched polyester with acetone in a mass ratio of 1 to 3:50, adding succinic anhydride of equal mass to the terminal hydroxyl hyperbranched polyester and catalyst triethylamine of 0.35 to 0.45 times the mass of the terminal hydroxyl hyperbranched polyester, heating to 58 to 62°C, reacting for 4 to 6 hours, precipitating with ethanolic sodium hydroxide solution and filtering, then washing with anhydrous ethanol for 3 to 5 times, and finally drying in vacuum at 50°C to obtain a carboxyl hyperbranched polyester; (5) mixing a carboxyl hyperbranched polyester and a vinyl glycol imidazole homopolymer in a mass ratio of 3 to 5:1, heating the mixture to 90 to 120° C., and adding concentrated sulfuric acid in an amount of 0.03 to 0.06 times the mass of the carboxyl hyperbranched polyester at a rate of 1 to 3 mL / min to obtain an ionic polymer; (6) PBT and glass fiber are dried at 60-70°C, and the dried PBT, dried glass fiber, homemade chain extender, ionic polymer and antioxidant 1010 are mixed in a mass ratio of 30:1-4:0.3-0.5:0.06:0.04, and extruded through a twin-screw extruder to obtain a high-strength plastic for automotive interior parts.
3. A method for preparing a high-strength plastic for automotive interior parts according to claim 2, It is characterized in that In the above step (1), the preparation method of the cyclohexylbenzamide matrix is as follows: trimesic acid, triphosgene and ethyl acetate are mixed in a mass ratio of 3.1-3.3:12:13, heated in a water bath to 25-28°C, initiator N,N-dimethylformamide in an amount of 0.45-0.55 times the mass of trimesic acid is added, and ethyl acetate in an amount of 0.8-0.9 times the mass of trimesic acid is added dropwise at a rate of 1-3 mL / min, the temperature is continued to be raised to 60-65°C, and the reaction is carried out for 7-8 hours to obtain the cyclohexylbenzamide matrix.
4. A method for preparing a high-strength plastic for automotive interior parts according to claim 2, It is characterized in that In the above step (2), the mass ratio of diphenyl chlorinated phosphate, triethylamine, 4-dimethylaminopyridine, neopentyl glycol, n-hexane and cyclohexylbenzamide is 10:1.5:3:1:4:5-7.
5. A method for preparing a high-strength plastic for automotive interior parts according to claim 2, It is characterized in that In the above step (3): the preparation method of vinyl glycol imidazole is: N-vinyl imidazole, bromoacetaldehyde ethylene glycol acetal and methanol are mixed in a mass ratio of 8-10:9:120, heated to 36-40°C in a water bath, stirred at 80-100 rpm for 20-40 min, heated to 52-56°C, continued to react for 4-6 h, cooled to room temperature and washed with ethyl acetate for 3-5 times, and rotary evaporated to obtain vinyl glycol imidazole.
6. A method for preparing a high-strength plastic for automotive interior parts according to claim 2, It is characterized in that In the above step (4): the preparation method of the terminal hydroxyl hyperbranched polyester is as follows: under a nitrogen atmosphere, trimethylolpropane, 2,2-dimethylolpropionic acid and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 1.1-1.3:9:0.1, the temperature is raised to 135-145°C, the temperature is reacted for 2-4 hours, the temperature is sealed and evacuated, the temperature is further reacted for 2-4 hours, the temperature is lowered to 40-50°C, the temperature is dissolved in acetone, and the temperature is precipitated with n-hexane, and finally the temperature is dried at 50-60°C to obtain the terminal hydroxyl hyperbranched polyester.