Composite diaphragm and preparation method thereof, and electrolysis device
By blasting and pre-evaporating the surface of the porous base film, a dense polymer layer is formed, which solves the problem of poor durability of composite separators in high-temperature and concentrated alkali environments, and achieves higher membrane strength and durability. At the same time, the use and cost increase of additional coatings are avoided.
Patent Information
- Application Number
- CN202410443089.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-12
AI Technical Summary
Traditional organic and inorganic composite separators have poor durability in high-temperature and concentrated alkali environments, and the surface coating is prone to fall off, resulting in a degradation of the separator performance.
The surface of the porous base film is blasted and/or light pre-evaporated by pre-evaporation to form a dense polymer layer, enhancing the overall strength and durability of the membrane and avoiding the use of additional coatings.
The durability and overall strength of the composite separator are improved, the possibility of inorganic hydrophilic powder falling off is reduced, the process is simplified and cost savings are saved.
Smart Images

Figure CN118207584B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrolysis technology, and in particular to a composite diaphragm and a preparation method thereof, and an electrolysis device. Background Art
[0002] Traditional alkaline water electrolysis technology uses polyphenylene sulfide (PPS) fabric diaphragm to separate the cathode and anode to block the crossover of hydrogen and oxygen, but this diaphragm has the problems of poor hydrophilicity, high impedance, and poor gas barrier ability. In response to this, the third-generation organic-inorganic composite diaphragm was developed. Compared with the PPS fabric diaphragm, this type of diaphragm has lower surface resistance and higher gas barrier ability, and is an important development direction for domestic alkaline water electrolysis hydrogen production diaphragms in the future. At present, the traditional preparation method of organic-inorganic composite diaphragms is mainly the non-solvent phase transformation method. However, the composite diaphragms prepared by this traditional method usually have the problem of poor durability. Summary of the invention
[0003] Based on this, the present application provides a composite diaphragm with better durability, a preparation method thereof, and an electrolysis device.
[0004] The first aspect of the present application provides a method for preparing a composite diaphragm, comprising:
[0005] Performing a pre-evaporation treatment on a porous base film coated with a polymer slurry on at least one side surface, wherein the pre-evaporation treatment includes air blowing pre-evaporation and / or light irradiation pre-evaporation;
[0006] The porous base membrane after the pre-evaporation treatment is immersed in a coagulation bath for phase inversion to form a polymer layer on at least one side surface of the porous base membrane to prepare the composite separator.
[0007] In some embodiments of the present application, at least one of the following conditions is met:
[0008] (1) The air blast pre-evaporation includes cold air pre-evaporation and / or hot air pre-evaporation;
[0009] (2) The light pre-evaporation includes infrared light and / or ultraviolet light.
[0010] In some embodiments of the present application, the pre-evaporation treatment includes air blast pre-evaporation and light irradiation pre-evaporation, and the light irradiation pre-evaporation is performed after the air blast pre-evaporation;
[0011] Optionally, the pre-evaporation treatment includes cold air pre-evaporation and ultraviolet light pre-evaporation.
[0012] In some embodiments of the present application, at least one of the following conditions is met:
[0013] (1) The air volume of the blast pre-evaporation is 50m³ / h~1000m³ / h;
[0014] (2) The air blast pre-evaporation time is 3s to 90s;
[0015] (3) The irradiation power of the light pre-evaporation is 100W~1000W;
[0016] (4) The light pre-evaporation time is 3 min to 10 min.
[0017] In some embodiments of the present application, the polymer slurry contains a polymer resin, an inorganic hydrophilic powder and an organic solvent.
[0018] In some embodiments of the present application, at least one of the following conditions is met:
[0019] (1) The polymer resin includes at least one of polysulfone, polyethersulfone, polyphenylsulfone, polyvinylidene fluoride, polymethyl methacrylate and copolymers thereof, and may be polysulfone and / or polyethersulfone;
[0020] (2) The inorganic hydrophilic powder includes at least one of zirconium oxide, hydrotalcite, titanium oxide, magnesium hydroxide and barium sulfate, and may be zirconium oxide and / or barium sulfate;
[0021] (3) The organic solvent includes at least one of dimethyl sulfoxide, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, N-benzylpyrrolidone and N-ethylpyrrolidone, and may be N-methylpyrrolidone and / or dimethylacetamide.
[0022] In some embodiments of the present application, at least one of the following conditions is met:
[0023] (1) The polymer slurry further comprises an additive;
[0024] Optionally, the additive includes at least one of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethylene oxide, polyethylene imine, polyethylene glycol, methyl cellulose, ethyl cellulose, polyvinylidene fluoride and polypropylene glycol, and polyvinyl pyrrolidone and / or polyethylene oxide may be selected;
[0025] (2) The porous base membrane comprises at least one of polyester porous fabric, polyphenylene sulfide porous fabric, polyurethane porous fabric, polyacrylonitrile porous fabric, polyetheretherketone porous fabric and sulfonated polyetheretherketone porous fabric, and can be polyphenylene sulfide porous fabric.
[0026] The second aspect of the present application provides a composite diaphragm, which is prepared by the preparation method described in the first aspect of the present application.
[0027] In some embodiments of the present application, the composite separator includes the porous base membrane and the polymer layer disposed on at least one surface of the porous base membrane.
[0028] The third aspect of the present application provides an electrolysis device, comprising the composite diaphragm described in the second aspect of the present application.
[0029] The composite diaphragm prepared by the preparation method of the present application has a more dense polymer surface layer formed on the surface of the porous base membrane. This structure can ensure the conductivity of ions inside the composite diaphragm, enhance the overall strength of the diaphragm, reduce the possibility of internal inorganic hydrophilic powder falling out from the pores on the surface of the diaphragm, and enhance the durability of the composite diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Surface morphologies of the composite membranes prepared in Examples 1 (Figure a), 3 (Figure b), 5 (Figure c) and Comparative Example 3 (Figure d).
[0031] Figure 2 This is a current density-voltage test curve diagram of the composite diaphragm prepared in Examples 1-5. DETAILED DESCRIPTION
[0032] In order to facilitate understanding of the present application, the present application will be described more comprehensively below. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0033] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. It should be noted that, unless otherwise specified, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" are inclusive of the number, and the meaning of "multiple" in "one or more" is more than two.
[0035] Herein, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values within the numerical interval is considered to be continuous and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval only refers to integers within the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.
[0036] In this article, if there are multiple steps involved in the method flow, unless there is a clear different description in this article, there is no strict order restriction for the execution of these steps, and they can be executed in other orders than described. Moreover, any step can include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn, alternating or simultaneously with other steps or parts of sub-steps or stages of other steps.
[0037] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0038] At present, the inorganic hydrophilic powder in the organic-inorganic composite diaphragm prepared by the traditional non-solvent phase conversion method is usually easy to fall off from the pores; and as the use time increases, the hydrophilicity of the diaphragm will gradually decrease, thereby increasing its area resistance, resulting in poor durability of the diaphragm. In order to improve this problem, there are currently plans to modify the surface coating of the composite diaphragm to improve its durability; for example, modify the surface of the composite diaphragm with a hydrophilic coating (such as a polyvinyl alcohol coating) to improve the powder shedding of the diaphragm, or coat the surface of the composite diaphragm to form a reinforcement layer (such as an epoxy resin layer) to improve the strength of the diaphragm.
[0039] However, composite diaphragms are often used in high-temperature, concentrated alkaline environments. Although the hydrophilic coating or the reinforcing layer has a certain degree of alkali resistance, it is not as good as the polymer resin (i.e., the organic part) used in the composite diaphragm itself. During the long-term use of the electrolytic cell, the surface coating is likely to react with the alkali, resulting in reduced strength and poor durability.
[0040] Moreover, when modifying the surface coating of the composite diaphragm, in addition to considering the performance of the surface coating, it is also necessary to consider the interfacial bonding force between the coating and the diaphragm itself. For example, the adhesion of polyvinyl alcohol is not strong enough. The long-term scouring of positive and negative electrode bubbles in the electrolytic cell environment, or the vibration of the cell itself, will cause the surface coating to fall off the surface of the diaphragm, ultimately resulting in poor durability of the diaphragm. At the same time, when modifying the surface coating of the composite diaphragm, it is also necessary to prepare an additional slurry for the diaphragm surface coating. The additional slurry requires more raw materials and process steps, and the material and time costs will be greatly increased.
[0041] In order to solve the aforementioned technical problems, the inventors proposed the following technical solutions of this application.
[0042] The first aspect of the present application provides a method for preparing a composite diaphragm, which may include the following steps:
[0043] S1, performing a pre-evaporation treatment on a porous base film coated with a polymer slurry on at least one side surface, wherein the pre-evaporation treatment includes air blowing pre-evaporation and / or light irradiation pre-evaporation;
[0044] S2. Immersing the pre-evaporation-treated porous base membrane in a coagulation bath for phase inversion to form a polymer layer on at least one side surface of the porous base membrane to prepare the composite membrane.
[0045] The above-mentioned preparation method provided by the present application, before phase inversion, the porous base film coated with polymer slurry is subjected to air blast pre-evaporation and / or light pre-evaporation. Wherein, when air blast pre-evaporation is performed, the effect of large air volume can increase the volatilization rate of the solvent in the polymer slurry, and cause the polymer in the slurry to produce pre-contraction, so that it is beneficial to shorten the subsequent phase inversion completion time, so that the porous base film surface quickly completes the phase inversion, and then it is beneficial to improve the compactness of the polymer layer generated by the phase inversion, so as to enhance the overall strength of the composite diaphragm. When light pre-evaporation is performed, the polymer slurry on the surface of the porous base film absorbs light energy, so that the polymer in the slurry can be pre-crosslinked, which is beneficial to form a cross-linked network structure with a higher degree of polymerization when the phase inversion is completed, and the cross-linking degree of the polymer layer is improved, so that the compactness of the polymer surface layer is improved, so as to enhance the overall strength of the composite diaphragm.
[0046] In addition, the inventors have discovered that when air pre-evaporation and light pre-evaporation are used in combination, there is a synergistic effect between the two. The synergistic effect of the two can quickly complete the phase transformation process on the surface of the polymer slurry, delay the entry of the non-solvent into the slurry, reduce the mutual solubility exchange between the non-solvent and the solvent, reduce the separation of the polymer and the solvent, and reduce the production of large-area uneven polymer-poor phases and polymer-rich phases caused by separation. This is conducive to the formation of a more uniform network structure inside the membrane, thereby further improving the density of the polymer layer and the durability of the composite diaphragm.
[0047] In this way, the composite diaphragm prepared by the preparation method of the present application generates a polymer surface layer with higher density on the surface of the porous base film. This structure can ensure the conductivity of ions inside the composite diaphragm, and can also strengthen the overall strength of the diaphragm, reduce the possibility of internal inorganic hydrophilic powder falling out of the pores on the surface of the diaphragm, and enhance its durability. Compared with the existing surface coating modification technology on the surface of the composite diaphragm, the present application improves the durability of the diaphragm by regulating the microstructure (i.e., the density of the polymer coating), without adding additional coatings on the surface of the composite diaphragm, the process is simple, cost-saving, and avoids the problems of insufficient alkali resistance and bonding strength of the coating.
[0048] It should be noted that, when performing pre-evaporation in the present application, only air blast pre-evaporation may be used, only light irradiation pre-evaporation may be used, or a combination of air blast pre-evaporation and light irradiation pre-evaporation may be used. Among them, when a combination of air blast pre-evaporation and light irradiation pre-evaporation is used, air blast pre-evaporation must be performed before light irradiation pre-evaporation.
[0049] The air blast pre-evaporation is carried out before the light irradiation pre-evaporation, which can make the polymer in the slurry pre-shrink better, thus further improving the density of the polymer layer.
[0050] In some embodiments, the forced air pre-evaporation includes cold air pre-evaporation and / or hot air pre-evaporation.
[0051] It can be understood that the "air blowing pre-evaporation" mentioned in this application refers to the pre-evaporation treatment by air blowing. Among them, "cold air pre-evaporation" means that the air applied during pre-evaporation is cold air, and its temperature is, for example, 0-25°C; "hot air pre-evaporation" means that the air applied during pre-evaporation is hot air, and its temperature is, for example, 25°C-60°C.
[0052] In some embodiments, the light irradiation pre-evaporation comprises infrared light irradiation and / or ultraviolet light irradiation.
[0053] In some embodiments, the pre-evaporation treatment includes air blowing pre-evaporation and light irradiation pre-evaporation, and the light irradiation pre-evaporation is performed after the air blowing pre-evaporation.
[0054] The inventors have discovered that when air blow pre-evaporation and light irradiation pre-evaporation are used simultaneously, there is a synergistic effect between the two. The synergistic effect of the two can complete the phase inversion process quickly and delay the entry of the non-solvent into the slurry, thereby further improving the density of the polymer layer and the durability of the composite diaphragm.
[0055] In some embodiments, the pre-evaporation treatment includes cold air pre-evaporation and ultraviolet light pre-evaporation.
[0056] In some embodiments, the air volume of the blast pre-evaporation is 50m³ / h to 1000m³ / h. For example, the air volume may be 50m³ / h, 100m³ / h, 150m³ / h, 300m³ / h, 500m³ / h, 700m³ / h, 1000m³ / h, or any range thereof.
[0057] In some embodiments, the air blast pre-evaporation time is 3s to 90s. For example, the time may be 3s, 5s, 10s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, or within a range of any of the above values.
[0058] In some embodiments, the irradiation power of the light pre-evaporation is 100 W to 1000 W. For example, the irradiation power may be 100 W, 200 W, 300 W, 400 W, 500 W, 600 W, 700 W, 800 W, 900 W, 1000 W, or any range thereof.
[0059] In some embodiments, the light pre-evaporation time is 3 min to 10 min. For example, the time can be 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min or any range thereof.
[0060] With the increase of blast volume, blast time, irradiation power and illumination time, the durability of composite diaphragm (such as abrasion loss rate and alkali resistance loss rate) will gradually increase. However, too long blast and illumination treatment will easily cause the composite diaphragm surface to pre-shrink strongly and the surface pore size to be too small, which is not conducive to the conduction of ions in the electrolytic cell. Therefore, a moderate intensity pre-evaporation treatment process, that is, regulating the blast volume, blast time, irradiation power or illumination time within the above respective ranges, can take into account the durability of the composite diaphragm and the conductivity of ions in the electrolytic cell.
[0061] In some embodiments, the polymer slurry comprises a polymer resin, an inorganic hydrophilic powder and an organic solvent.
[0062] In some embodiments, the polymer resin includes at least one of polysulfone (PSU), polyethersulfone (PES), polyphenylsulfone (PPSU), polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA) and copolymers thereof, and may be polysulfone and / or polyethersulfone.
[0063] It is understood that the "and copolymers thereof" mentioned in the present application refer to copolymers obtained by polymerizing two or more different polymer resins, for example, copolymers formed by polymerizing polysulfone and polyethersulfone, copolymers formed by polymerizing polysulfone, polyethersulfone and polyphenylsulfone, etc.
[0064] In some embodiments, the inorganic hydrophilic powder includes at least one of zirconium oxide, hydrotalcite, titanium oxide, magnesium hydroxide and barium sulfate, and may be zirconium oxide and / or barium sulfate.
[0065] In some embodiments, the organic solvent includes at least one of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), N-methylpyrrolidone (NMP), N-benzylpyrrolidone (NBP) and N-ethylpyrrolidone (NEP), and may be N-methylpyrrolidone and / or dimethylacetamide.
[0066] In some embodiments, the polymer slurry further comprises an additive. During the phase inversion process, the additive can be separated from the polymer slurry and dissolved in water, and small holes can be formed at the original location of the additive, which is conducive to forming a porous network structure of the polymer layer.
[0067] In some embodiments, the additive includes at least one of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), polyvinyl acetate (PVAC), polyethylene oxide (PEO), polyethylene imine (PEI), polyethylene glycol, methyl cellulose, ethyl cellulose, polyvinylidene fluoride (PVDF) and polypropylene glycol, and polyvinyl pyrrolidone and / or polyethylene oxide may be selected.
[0068] In some embodiments, the porous base membrane includes at least one of polyester (PET) porous fabric, polyphenylene sulfide (PPS) porous fabric, polyurethane (PU) porous fabric, polyphenylene nitrile (PAN) porous fabric, polyetheretherketone (PEEK) porous fabric and sulfonated polyetheretherketone (SPEEK) porous fabric, and can be polyphenylene sulfide porous fabric.
[0069] The second aspect of the present application provides a composite diaphragm, which is prepared by the preparation method of the first aspect of the present application.
[0070] In some embodiments, the composite separator includes the porous base membrane and the polymer layer disposed on at least one surface of the porous base membrane.
[0071] The third aspect of the present application provides an electrolysis device, comprising the composite diaphragm of the second aspect of the present application.
[0072] In some embodiments, the electrolysis device may be a device for electrolyzing water, a device for electrolyzing carbon dioxide, or a device for electrolyzing or electrolyzing chlorine-alkali.
[0073] Example
[0074] The following are specific examples, which more specifically describe the contents disclosed in this application, and these examples are only for illustrative purposes, because it is obvious to those skilled in the art that various modifications and variations are made within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0075] Example 1
[0076] S1. Add NMP, PSU, ZrO2 and PVP into a vacuum mixer, where the mass ratio of the four substances is 40:20:35:5. Stir at a speed of 2000r / min at room temperature and pressure until completely dissolved, then stand to degas to form a milky white precursor slurry. Pour the slurry onto a slit coater, and control the slit width to 500μm. Use PPS fabric to pass through the slit and evenly apply a layer of slurry on its opposite sides (i.e., the front and back sides).
[0077] S2. Use an industrial blower with an air volume of 50m³ / h to blow air to the front and back sides of the PPS fabric coated with slurry for 3 seconds at the same time, then place it between two UV lamps and irradiate the front and back sides for 3 minutes at the same time for pre-evaporation. The power of the UV lamp is 100W.
[0078] S3. Immerse the pre-evaporated PPS fabric in water to complete phase inversion, and form a polymer layer on the front and back surfaces of the PPS fabric to obtain a composite diaphragm.
[0079] Example 2
[0080] The preparation method is similar to that of Example 1, except that step S2 is replaced by:
[0081] Use an industrial blower with an air volume of 300m³ / h to blow air to the front and back sides of the PPS fabric coated with slurry for 40 seconds at the same time, then place it between two UV lamps and irradiate the front and back sides for 5 minutes for pre-evaporation. The power of the UV lamp is 500W.
[0082] Example 3
[0083] The preparation method is similar to that of Example 1, except that step S2 is replaced by:
[0084] Use an industrial blower with an air volume of 1000m³ / h to blow air on both sides of the PPS fabric coated with slurry for 90s, then place it between two UV lamps and irradiate both sides for 10min for pre-evaporation. The power of the UV lamp is 1000W.
[0085] Example 4
[0086] The preparation method is similar to that of Example 1, except that step S2 is replaced by:
[0087] Use an industrial blower with an air volume of 1000m³ / h to blow air on both sides of the PPS fabric coated with slurry for 120s, then place it between two UV lamps and irradiate both sides for 15min for pre-evaporation. The power of the UV lamp is 1000W.
[0088] Example 5
[0089] The preparation method is similar to that of Example 1, except that step S2 is replaced by:
[0090] An industrial blower with an air volume of 1000m³ / h was used to blow air to the front and back sides of the PPS fabric coated with the slurry for 150s at the same time, and then it was placed between two UV lamps and irradiated on the front and back sides for 20 minutes for pre-evaporation. The power of the UV lamp was 1000W.
[0091] Example 6
[0092] The preparation method is similar to that of Example 3, except that the NMP in step S1 is replaced by an equal mass of DMAc.
[0093] Example 7
[0094] The preparation method is similar to that of Example 3, with the main difference being that the PSU in step S1 is replaced by PES of equal mass.
[0095] Example 8
[0096] The preparation method is similar to that of Example 3, with the main difference being that the ZrO2 in step S1 is replaced by an equal mass of BaSO4.
[0097] Example 9
[0098] The preparation method is similar to that of Example 3, the main difference being that the PVP in step S1 is replaced by an equal mass of polyethylene oxide.
[0099] Example 10
[0100] The preparation method is similar to that of Example 3, with the main difference being that in step S1, the slit width is controlled to be 700 μm.
[0101] Comparative Example 1
[0102] The preparation method is similar to that of Example 3, except that, in the pre-evaporation in step S2, only an industrial blower with an air volume of 1000 m³ / h is used to blow air to the front and back sides of the PPS fabric coated with the slurry for 90 seconds at the same time, and the ultraviolet irradiation is omitted.
[0103] Comparative Example 2
[0104] The preparation method is similar to that of Example 3, with the main difference being that, in the pre-evaporation in step S2, the PPS fabric coated with the slurry is only placed between two UV lamps and irradiated on both sides for 10 minutes, the power of the UV lamp is 1000 W, and the air blowing operation is omitted.
[0105] Comparative Example 3
[0106] The preparation method is similar to that of Example 3, with the main difference being that in step S2, the PPS fabric coated with the slurry is placed in the air for pre-evaporation, and the air blowing operation and the irradiation with the ultraviolet lamp are omitted.
[0107] The composite membranes prepared in Examples 1 to 10 and Comparative Examples 1 to 3 were subjected to relevant performance tests, and the test results are shown in Table 1 below.
[0108] Among them, the test conditions or test standards for each performance test item are as follows:
[0109] (1) Wear loss rate:
[0110] The samples were cut into 5 specimens of (70±0.2)×(70±0.2) mm.
[0111] Place the sample in an oven at 100°C and dry it for 2 h, then take it out and weigh its dry mass W1.
[0112] The sample was fixed on the testing machine, and a 1×1 cm friction head was selected. The friction head was completely wrapped with 800-mesh sandpaper and run 60 times at a friction frequency of 50 times / min and a friction stroke of 60 mm.
[0113] After the test, place it in a 100℃ oven to dry for 2 h, take it out and weigh its dry mass W2.
[0114] Substitute the test results into the calculation formula (1) to calculate the wear loss rate. Take the arithmetic mean of the five wear loss rates as the test result.
[0115] (1)
[0116] Where:
[0117] E is the wear loss rate of the sample, %;
[0118] W1 is the dry mass of the sample before abrasion, g;
[0119] W2 is the dry mass of the sample after abrasion, g.
[0120] (2) Alkali resistance loss rate:
[0121] Cut the sample into 5 specimens of (100±0.2) mm×(100±0.2) mm.
[0122] After the sample is fully dried in an oven at 100°C for 2 h, it is taken out and placed in a glass drying dish to cool to room temperature, and then its mass W1 is weighed on a balance.
[0123] The sample was immersed in a 30% potassium hydroxide solution at 120°C. After 400 h, the sample was taken out and washed with deionized water until it was neutral (checked with phenolphthalein indicator).
[0124] Place the washed neutral sample in an oven at 100°C for 2 h, place it in a glass drying dish to cool to room temperature, and then weigh its mass W2 on a balance.
[0125] Substitute the test results into the calculation formula (2) to calculate the alkali resistance loss rate. Take the arithmetic mean of the 5 samples as the test result.
[0126] (2)
[0127] Where:
[0128] E is the alkali resistance loss rate of the sample, %;
[0129] W1 is the mass of the sample before alkali immersion, g;
[0130] W2 is the mass of the sample after alkali immersion, g.
[0131] (3) Surface morphology test:
[0132] The surface morphology of the composite membrane was observed using a scanning electron microscope (SEM).
[0133] (4) Current density-voltage test:
[0134] This shall be carried out in accordance with the provisions of 6.2.2.3 of GB / T 19774-2005.
[0135] Table 1
[0136]
[0137] In Table 1 above, it can be seen from the comparison of Examples 1-5 that with the increase of the blast air volume, the extension of the blast time, the increase of the UV lamp power, and the extension of the UV irradiation time during the pre-evaporation process, the wear loss rate and the alkali resistance loss rate of the composite diaphragm gradually decreased. However, too long a blast and UV irradiation treatment will increase the energy consumption of the diaphragm (e.g. Figure 2 This is because the composite membrane surface has strong pre-shrinkage and the surface pore size is too small, which is not conducive to the conduction of ions in the electrolytic cell. Therefore, a moderate intensity pre-evaporation treatment process can take into account the durability of the membrane and the energy consumption performance in the electrolytic cell.
[0138] Comparing Example 3 and Example 6, it can be seen that after the solvent is replaced by DMAc from NMP, the abrasion loss rate and alkali resistance loss rate are reduced. This is because DMAc is more volatile than NMP under the action of air blast, and the pre-shrinkage of the slurry surface is more significant. However, DMAc is less soluble in polysulfone than NMP, and it takes longer to dissolve.
[0139] Comparing Example 3 and Example 7, it can be seen that after the polymer resin is replaced by PES from PSU, the abrasion loss rate and alkali resistance loss rate are reduced. This is because PES has more active groups, and under the condition of ultraviolet light, it undergoes stronger pre-crosslinking, and the surface of the diaphragm is denser after phase transformation.
[0140] By comparing Example 3 with Examples 8-9, it can be seen that the abrasion loss rate and alkali resistance loss rate change little when the inorganic hydrophilic powder and additives in the slurry are replaced, indicating that the replacement of the inorganic hydrophilic powder and additives is still suitable for the processes of air pre-evaporation and UV pre-evaporation.
[0141] Comparing Example 3 and Example 10, it can be seen that when the slit width is increased from 500 μm to 700 μm, the loss rate and alkali resistance loss rate are increased. This is because the total amount of slurry increases after the slit width is increased, and under the same air blast and ultraviolet irradiation process conditions, the pre-shrinkage and cross-linking degree of the diaphragm surface decrease. Therefore, when the slit width changes, the intensity of subsequent air blast and ultraviolet irradiation should also be reduced or increased accordingly.
[0142] By comparing Example 3 and Comparative Examples 1-2, it can be seen that the use of air pre-evaporation or ultraviolet light pre-evaporation alone can also improve the reduction of the diaphragm wear loss rate and alkali resistance loss rate, but the effect is better when the two methods are used at the same time, which is due to the synergistic effect.
[0143] By comparing Examples 1-5, Comparative Examples 1-2 and Comparative Example 3, it can be seen that after air blast pre-evaporation and ultraviolet light pre-evaporation, the mass loss rate of the diaphragm is lower than that of conventional air pre-evaporation, indicating that it has higher mechanical strength and better durability.
[0144] In addition, from Figure 1 It can be seen that when conventional air pre-evaporation is used (Comparative Example 3), the diaphragm exhibits a rough surface ( Figure 1 d). When air blowing and UV light irradiation are used simultaneously during the pre-evaporation process (Example 1), the pore size of the membrane surface decreases ( Figure 1 a). After increasing the air volume of the blower and extending the blowing time while increasing the UV lamp power and UV irradiation time (Example 3), the pore size of the membrane surface is further reduced, forming a denser surface ( Figure 1 b). When the pre-evaporation process is performed with a blower air volume of 1000 m³ / h, a time of 150 s, a UV lamp power of 1000 w, and a time of 20 min (Example 5), the through holes on the surface of the diaphragm disappear, forming a dense surface ( Figure 1 c).
[0145] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0146] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for preparing a composite diaphragm, characterized in that: include: Performing a pre-evaporation treatment on a porous base film coated with a polymer slurry on at least one side surface, wherein the pre-evaporation treatment includes air blast pre-evaporation and light irradiation pre-evaporation, wherein the light irradiation pre-evaporation is performed after the air blast pre-evaporation; The porous base membrane after the pre-evaporation treatment is immersed in a coagulation bath for phase inversion to form a polymer layer on at least one side surface of the porous base membrane to prepare the composite separator.
2. The preparation method according to claim 1, characterized in that: Satisfy at least one of the following conditions: (1) The air blast pre-evaporation includes cold air pre-evaporation and / or hot air pre-evaporation; (2) The light pre-evaporation includes infrared light and / or ultraviolet light.
3. The preparation method according to claim 2, characterized in that: The pre-evaporation treatment includes the cold air pre-evaporation and the ultraviolet light pre-evaporation.
4. The preparation method according to any one of claims 1 to 3, characterized in that Satisfy at least one of the following conditions: (1) The air volume of the blast pre-evaporation is 50m 3 / h~1000m 3 / h; (2) The air blast pre-evaporation time is 3s to 90s; (3) The irradiation power of the light pre-evaporation is 100W to 1000W; (4) The time of the light pre-evaporation is 3 minutes to 10 minutes.
5. The preparation method according to any one of claims 1 to 3, characterized in that: The polymer slurry contains high molecular resin, inorganic hydrophilic powder and organic solvent.
6. The preparation method according to claim 5, characterized in that: Satisfy at least one of the following conditions: (1) The polymer resin includes at least one of polysulfone, polyethersulfone, polyphenylsulfone, polyvinylidene fluoride, polymethyl methacrylate and copolymers thereof; (2) the inorganic hydrophilic powder comprises at least one of zirconium oxide, hydrotalcite, titanium oxide, magnesium hydroxide and barium sulfate; (3) The organic solvent includes at least one of dimethyl sulfoxide, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, N-benzylpyrrolidone and N-ethylpyrrolidone.
7. The preparation method according to claim 6, characterized in that: Satisfy at least one of the following conditions: (1) The polymer resin is polysulfone and / or polyethersulfone; (2) The inorganic hydrophilic powder is zirconium oxide and / or barium sulfate; (3) The organic solvent is N-methylpyrrolidone and / or dimethylacetamide.
8. The preparation method according to claim 5, characterized in that: Satisfy at least one of the following conditions: (1) The polymer slurry further comprises an additive; (2) The porous base membrane comprises at least one of polyester porous fabric, polyphenylene sulfide porous fabric, polyurethane porous fabric, polyacrylonitrile porous fabric, polyetheretherketone porous fabric and sulfonated polyetheretherketone porous fabric.
9. The preparation method according to claim 8, characterized in that: The additive includes at least one of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethylene oxide, polyethylene imine, polyethylene glycol, methyl cellulose, ethyl cellulose, polyvinylidene fluoride and polypropylene glycol.
10. The preparation method according to claim 9, characterized in that: The additive is polyvinyl pyrrolidone and / or polyethylene oxide.
11. The preparation method according to claim 8, characterized in that: The porous base membrane is a polyphenylene sulfide porous fabric.
12. A composite diaphragm, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 11.
13. The composite diaphragm according to claim 12, characterized in that: The invention comprises the porous base membrane and the polymer layer arranged on at least one surface of the porous base membrane.
14. An electrolysis device, characterized in that: Comprising the composite diaphragm according to claim 12 or 13.
Citation Information
Patent Citations
Coating slurry of electrolyzed water composite membrane and preparation method of composite membrane
CN115772683A
Super-hydrophilic alkaline water electrolyser composite diaphragm and preparation method thereof
CN117248240A
Composite diaphragm with super-hydrophilic surface and integral cross-linked structure for hydrogen production by alkaline water electrolysis and preparation method of composite diaphragm
CN117512693A
Preparation method of polysulfone / inorganic composite diaphragm for alkaline electrolyzed water
CN117702183A
High-hydrophilicity and low-resistance composite diaphragm for hydrogen production by alkaline water electrolysis and preparation method of high-hydrophilicity and low-resistance composite diaphragm
CN117721497A