Method for converting paint waste residue into paint anti-corrosion material
Through multi-component solvent stirring and oxidation treatment under acidic environment, combined with amidation reaction, the paint waste slag is successfully converted into high-quality paint anticorrosion materials, solving the problems of degradation of quality and high cost in paint waste slag treatment, and achieving strong functional And widely used paint anticorrosion materials.
Patent Information
- Application Number
- CN202410552030.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-07
AI Technical Summary
It is difficult to achieve functional conversion of paint waste slag treatment, resulting in a decrease in paint quality and high cost and time investment, making it difficult to control the chemical composition and functional properties of waste slag.
After stirring and dissolving with a multi-component solvent, filter impurities, mix glacial acetic acid, sulfuric acid, metal oxides and oxidants, introduce carboxylic acid groups and catechol groups, and form a modified paint waste system through amidation reaction, which is used to prepare Paint anticorrosion material.
It improves the quality of the paint waste residue reuse products, has high adaptability, is simple to prepare and low cost, and enhances the barrier properties and scope of application of anticorrosion materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of paint waste treatment, in particular to a method for converting paint waste residue into paint anti-corrosion material. Background Art
[0002] Paint waste is a type of waste generated during the construction, production or treatment of paint. Its main components include resins, solvents, pigments, etc. These wastes are classified as hazardous wastes because they usually have dangerous characteristics such as toxicity and flammability. If not handled properly, they may cause serious pollution and harm to the environment.
[0003] Paint waste contains a large amount of organic materials, which can be recycled and reused to prepare new paint or as paint components. Paints made from recycled paint waste often have quality problems compared to original paints. After the recycled paint waste is re-dissolved, some substances produced by the breakage of polymers in it can no longer participate in the reaction of paint preparation, but exist in the paint in the form of "impurities", resulting in unstable paint performance or quality degradation, thereby limiting the application scope of paint waste.
[0004] Recycling paint waste residues as functional components such as anti-corrosion materials and hardness fillers, and then investing them in paint preparation is also a promising research direction. However, due to the complex chemical composition of paint waste residues, it is difficult to have a unified treatment method to treat the waste residues. In addition, since the content of each component in the waste residues is difficult to control, waste residues from different sources have different chemical properties, so it is difficult to fix the properties of the obtained functions. Qualitative and quantitative testing of the components of paint waste residues before each production requires greater costs and time, which is difficult to achieve in actual production. Therefore, a new method for treating paint waste residues is needed to convert them into materials with strong functionality without reducing the quality of paint. Summary of the invention
[0005] The object of the present invention is to provide a method for converting paint waste residue into paint anticorrosive materials to solve the problems raised in the background technology. The paint waste is stirred and dissolved using a multi-component solvent, and a small amount of impurities that are severely aged and cannot be dissolved are filtered out for subsequent mixing with anticorrosive materials to improve the barrier properties of the anticorrosive materials. The obtained filtrate is then mixed with glacial acetic acid, sulfuric acid, metal oxides and oxidant components, and carboxylic acid oxygen-containing groups are introduced into the system using composite acids and metal oxide catalysts. And by amidation of the carboxylic acid group, catechol groups are introduced into the system, so that the paint waste system can be applied to more types of compound paints, fillers and substrates. The prepared paint anticorrosive material has the characteristics of high adaptability, simple preparation and low cost, which effectively improves the quality of the paint waste residue recycling product.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0008] S1. Collecting paint waste, drying at 50-80°C, dissolving the paint waste residue with a waste solvent, homogenizing and filtering, collecting the filtrate and the filtrate; grinding, crushing and sieving the filtrate after drying to obtain component A, and storing it for standby use;
[0009] S2, add glacial acetic acid, sulfuric acid, metal oxide and oxidant to the filtrate obtained in step S1, stir evenly, raise the system temperature to 60-90°C, stir and react for 0.5-3 hours, then cool to room temperature, filter the system, let the filtrate stand and separate, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0010] S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system;
[0011] S4, removing water from the modified waste system, and finally mixing it with component A obtained in step S1 and component B obtained in step S2, stirring evenly and then mixing it with the reinforcing material in any ratio to obtain a paint anti-corrosion material.
[0012] Furthermore, a method for converting paint waste residue into paint anti-corrosion material comprises the following steps:
[0013] S1. Collect paint waste, dry at 50-80°C, take (10-30) g, use 100 mL of waste solvent to dissolve paint waste residue, homogenize at a pressure of 20 MPa, filter, collect the filtrate and the filtrate; after drying, grind, crush, and pass through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0014] S2, add glacial acetic acid, sulfuric acid, metal oxide and oxidant to 300 mL of the filtrate obtained in step S1, stir evenly, raise the system temperature to 60-90°C, stir and react at a rate of 30 rpm for 0.5-3 hours, then cool to room temperature, filter the system, and let the filtrate stand for stratification, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0015] In the above reaction process, after the paint waste is dissolved in the solvent, it contains a large amount of aromatic hydrocarbons. When the system is treated with an oxidant in an acidic environment, the aromatic hydrocarbon side chain can be oxidized. When the α-carbon atom of the aromatic ring contains a hydrogen atom, an aromatic carboxylic acid is finally generated under the action of a strong oxidant. Due to the large amount of oxidant used, a small amount of hydroxyl contained in the system will also be oxidized to carboxylic acid. In the process, the metal oxide used as a catalyst reduces the activation energy of the reaction, making the reaction easier to proceed.
[0016] S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system;
[0017] S4. Wash the modified waste system with saturated brine, use a desiccant to remove moisture, and then mix it with component A obtained in step S2 and component B obtained in step S2. After stirring evenly, mix it with the reinforcing material in any ratio to obtain a paint anti-corrosion material.
[0018] Furthermore, in step S1, the waste solvent is obtained by mixing alcohols, esters and aromatic hydrocarbons.
[0019] Furthermore, the ester is at least one of ethyl acetate and butyl butyrate, and the aromatic hydrocarbon is at least one of toluene and xylene.
[0020] Furthermore, the waste solvent is obtained by mixing ethanol, ethyl acetate and xylene in a mass ratio of (1-3): (0.1-2):5.
[0021] Furthermore, in step S2, the volume mass ratio of the filtrate to glacial acetic acid, sulfuric acid solution, metal oxide and oxidant is 300 mL: (50-80) mL: (10-20) mL: (5-10) g: (10-30) g, wherein the sulfuric acid is a 40-70 wt% sulfuric acid solution; the oxidant is at least one of potassium permanganate, hydrogen peroxide, hypochlorite, potassium dichromate, sodium periodate or nitric acid; and the metal oxide is at least one of chromium trioxide, cupric oxide and ferrous oxide.
[0022] Further, in step S3, the modified waste system is specifically prepared by the following steps:
[0023] 2-Morpholineethanesulfonic acid is added to the waste system, and the pH value of the system is adjusted to 5.1. Subsequently, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride are added to the system, and the reaction is stirred for 5-10 hours under an inert atmosphere to obtain a modified waste system.
[0024] Further, in step S3, the modified waste system is specifically prepared by the following steps:
[0025] A 0.1 mol / L 2-morpholineethanesulfonic acid solution was added to the waste system at a mass ratio of (0.2-0.7):400, and a 0.1 mol / L NaOH solution was used to adjust the pH value of the system to 5.1. Subsequently, 0.192 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (hereinafter referred to as EDC), 0.115 g of N-hydroxysuccinimide (hereinafter referred to as NHS) and dopamine hydrochloride were added to the system, and the reaction was stirred for 5-10 hours under an inert atmosphere to obtain a modified waste system.
[0026] In the above reaction process, the carboxyl groups in the modified waste system and the carboxyl groups on dopamine hydrochloride are subjected to amidation reaction using EDC / NHS, and catechol groups are introduced into the waste system to prepare the modified waste system.
[0027] Furthermore, the mass ratio of the waste system to dopamine hydrochloride is 400:(0.5-5.0).
[0028] Furthermore, in step S4, the anticorrosive material is at least one of graphene, SiO2, an inorganic amphoteric compound, a metal powder and a zinc salt. The amphoteric compound is at least one of zinc hydroxide, aluminum hydroxide, aluminum oxide, copper hydroxide and barium hydroxide.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] In the technical solution of the present invention, the paint waste is stirred and dissolved using a multi-component solvent, and a small amount of impurities that are severely aged and cannot be dissolved are filtered out for subsequent mixing with anti-corrosion materials to improve the barrier properties of the anti-corrosion materials.
[0031] The obtained filtrate is then mixed with glacial acetic acid, sulfuric acid, metal oxide and oxidant components. In an acidic environment, the system can be treated with an oxidant to oxidize the side chain of aromatic hydrocarbons, and when the α-carbon atom of the aromatic ring contains a hydrogen atom, an aromatic carboxylic acid is finally generated under the action of a strong oxidant. Due to the large amount of oxidant used, a small amount of hydroxyl groups contained in the system will also be oxidized to carboxylic acids. In the process, the metal oxide used is used as a catalyst to reduce the activation energy of the reaction, making the reaction easier to proceed. A large amount of oxidant used can also oxidize the alcohol in the system to carboxylic acids to increase the content of carboxyl groups in the system.
[0032] Subsequently, the carboxyl groups contained in the system are used to carry out an amidation reaction. Under the conditions of EDC / NHS, the amino group reacts specifically with the carboxyl groups in the system without affecting other groups. As the grafting is completed, in the subsequent mixing process, the metal catalyst used can be distributed in the system in the form of a metal ion coordination bond with the catechol group. Subsequently, an anticorrosive material is added to the system, and a paint anticorrosive material is prepared after blending. The prepared paint anticorrosive material can be compounded with a variety of paint systems containing benzene rings and fatty acid chains, and in the paint, it can have good coverage and adhesion effects on various planes such as inorganic solids composed of silicates and metals. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0036] S1. Ethanol, ethyl acetate and xylene are mixed in a mass ratio of 1:0.1:5 to obtain a waste solvent; paint waste is collected, and after baking at 50°C for 2 hours, 10 g of the waste is taken and 100 mL of the waste solvent is used to dissolve the paint waste residue, and the waste is homogenized at a pressure of 20 MPa and then filtered, and the filtrate and the filtrate are collected; the filtrate is dried, ground, crushed, and sieved through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0037] S2, to 300 mL of the filtrate obtained in step S1, add 50 mL of glacial acetic acid, 10 mL of 40 wt% sulfuric acid, 5 g of chromium trioxide and 10 g of potassium permanganate, stir evenly, raise the system temperature to 60 ° C, stir at 30 rpm for 0.5 hours, then cool to room temperature, filter the system, and let the filtrate stand for stratification, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0038] S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system: the specific operation is:
[0039] 0.2 g of 0.1 mol / L 2-morpholineethanesulfonic acid solution was added to 400 g of the waste system obtained in step S2, and the pH value of the system was adjusted to 5.1 using 0.1 mol / L NaOH solution, and then 0.192 g of EDC, 0.115 g of NHS and 0.5 g of dopamine hydrochloride were added to the system, and the mixture was stirred and reacted for 5 hours under a nitrogen atmosphere to obtain a modified waste system;
[0040] S4. After washing the modified waste system with saturated brine, treat it with anhydrous magnesium sulfate desiccant to remove moisture, and then mix it with component A obtained in step S2 and component B obtained in step S2. After stirring evenly, mix it with 10g of SiO2 powder with a particle size of 50±5nm and a purity of 99.5% to obtain a paint anti-corrosion material.
[0041] Example 2
[0042] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0043] S1. Ethanol, ethyl acetate and xylene are mixed in a mass ratio of 2:1:5 to obtain a waste solvent; paint waste is collected, and after baking at 60°C for 2 hours, 20 g of the waste is taken and dissolved in 100 mL of the waste solvent, and the waste paint residue is homogenized at a pressure of 20 MPa and then filtered, and the filtrate and the filtrate are collected; the filtrate is dried, ground, crushed, and sieved through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0044] S2, to 300 mL of the filtrate obtained in step S1, add 60 mL of glacial acetic acid, 10 mL of 50 wt% sulfuric acid, 12 g of chromium trioxide and 20 g of potassium permanganate, stir evenly, raise the system temperature to 70 ° C, stir at 30 rpm for 1.5 hours, then cool to room temperature, filter the system, and let the filtrate stand for stratification, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0045] S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system: the specific operation is:
[0046] 0.5 g of 0.1 mol / L 2-morpholineethanesulfonic acid solution was added to 400 g of the waste system, and the pH value of the system was adjusted to 5.1 using 0.1 mol / L NaOH solution. Subsequently, 0.192 g of EDC, 0.115 g of NHS and 2.7 g of dopamine hydrochloride were added to the system, and the mixture was stirred and reacted for 8 hours under a nitrogen atmosphere to obtain a modified waste system.
[0047] S4. After washing the modified waste system with saturated brine, treat it with anhydrous magnesium sulfate desiccant to remove moisture, and then mix it with component A obtained in step S2 and component B obtained in step S2. After stirring evenly, mix it with 10g of SiO2 powder with a particle size of 50±5nm and a purity of 99.5% to obtain a paint anti-corrosion material.
[0048] Example 3
[0049] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0050] S1. Ethanol, butyl butyrate and toluene are mixed in a mass ratio of 3:2:5 to obtain a waste solvent; paint waste is collected, and after baking at 80°C for 2 hours, 30 g of the paint waste is dissolved in 100 mL of the waste solvent, and the paint waste residue is homogenized at a pressure of 20 MPa and then filtered, and the filtrate and the filtrate are collected; the filtrate is dried, ground, crushed, and sieved through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0051] S2, add 80 mL of glacial acetic acid, 20 mL of 70 wt% sulfuric acid, 10 g of copper oxide and 30 g of sodium periodate to 300 mL of the filtrate obtained in step S1, stir evenly, raise the system temperature to 90 ° C, stir at 30 rpm for 3 hours, then cool to room temperature, filter the system, and let the filtrate stand for stratification, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0052] S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system: the specific operation is:
[0053] 0.7 g of 0.1 mol / L 2-morpholineethanesulfonic acid solution was added to 400 g of the waste system, and the pH value of the system was adjusted to 5.1 using 0.1 mol / L NaOH solution. Subsequently, 0.192 g of EDC, 0.115 g of NHS and 5.0 g of dopamine hydrochloride were added to the system, and the mixture was stirred and reacted for 10 hours under a nitrogen atmosphere to obtain a modified waste system.
[0054] S4. After washing the modified waste system with saturated brine, use anhydrous magnesium sulfate desiccant to remove moisture, then mix it with component A obtained in step S2 and component B obtained in step S2, stir evenly and mix it with 10g of aluminum hydroxide powder with a particle size of 1μm and a purity of 99.8% to obtain a paint anti-corrosion material.
[0055] Comparative Example 1
[0056] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0057] S1. Ethanol, ethyl acetate and xylene are mixed in a mass ratio of 2:1:5 to obtain a waste solvent; paint waste is collected, and after baking at 60°C for 2 hours, 20 g of the waste is taken and dissolved in 100 mL of the waste solvent, and the waste paint residue is homogenized at a pressure of 20 MPa and then filtered, and the filtrate and the filtrate are collected; the filtrate is dried, ground, crushed, and sieved through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0058] S2. Wash the filtered material with saturated brine, use anhydrous magnesium sulfate desiccant to remove moisture, then mix it with component A obtained in step S1, stir it evenly and mix it with 10g SiO2 powder with a particle size of 50±5nm and a purity of 99.5% to obtain a paint anti-corrosion material.
[0059] Comparative Example 2
[0060] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0061] S1. Ethanol, ethyl acetate and xylene are mixed in a mass ratio of 2:1:5 to obtain a waste solvent; paint waste is collected, and after baking at 60°C for 2 hours, 20 g of the waste is taken and dissolved in 100 mL of the waste solvent, and the waste paint residue is homogenized at a pressure of 20 MPa and then filtered, and the filtrate and the filtrate are collected; the filtrate is dried, ground, crushed, and sieved through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0062] S2, to 300 mL of the filtrate obtained in step S1, add 60 mL of glacial acetic acid, 10 mL of 50 wt% sulfuric acid, 12 g of chromium trioxide and 20 g of potassium permanganate, stir evenly, raise the system temperature to 70 ° C, stir at 30 rpm for 1.5 hours, then cool to room temperature, filter the system, and let the filtrate stand for stratification, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0063] S3. Wash the waste system with saturated brine, treat it with anhydrous magnesium sulfate desiccant to remove moisture, and then mix it with component A obtained in step S2 and component B obtained in step S2. After stirring evenly, mix it with 10g of SiO2 powder with a particle size of 50±5nm and a purity of 99.5% to obtain a paint anti-corrosion material.
[0064] Comparative Example 3
[0065] A method for converting paint waste residue into paint anti-corrosion materials, comprising the following steps:
[0066] S1. Ethanol, ethyl acetate and xylene are mixed in a mass ratio of 2:1:5 to obtain a waste solvent; paint waste is collected, and after baking at 60°C for 2 hours, 20 g of the waste is taken and dissolved in 100 mL of the waste solvent, and the waste paint residue is homogenized at a pressure of 20 MPa and then filtered, and the filtrate and the filtrate are collected; the filtrate is dried, ground, crushed, and sieved through a 100-mesh sieve to obtain component A, which is stored for standby use;
[0067] S2, add 10mL 50wt% sulfuric acid and 20g potassium permanganate to 300mL of the filtrate obtained in step S1, stir evenly, raise the system temperature to 70°C, stir and react at a rate of 30rpm for 1.5 hours, then cool to room temperature, filter the system, and let the filtrate stand for stratification, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system;
[0068] S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system: the specific operation is:
[0069] 0.5 g of 0.1 mol / L 2-morpholineethanesulfonic acid solution was added to 400 g of the waste system, and the pH value of the system was adjusted to 5.1 using 0.1 mol / L NaOH solution. Subsequently, 0.192 g of EDC, 0.115 g of NHS and 2.7 g of dopamine hydrochloride were added to the system, and the mixture was stirred and reacted for 8 hours under a nitrogen atmosphere to obtain a modified waste system.
[0070] S4. After washing the modified waste system with saturated brine, use anhydrous magnesium sulfate desiccant to remove moisture, then mix it with component A obtained in step S2, 12g of chromium trioxide and component B obtained in step S2, stir evenly and mix it with 10g of SiO2 powder with a particle size of 50±5nm and a purity of 99.5% to obtain a paint anti-corrosion material.
[0071] The anti-corrosion effect of the paint anti-corrosion materials prepared in Examples 1-3 and Comparative Examples 1-3 was tested. 10 g of the paint anti-corrosion materials prepared in different groups were mixed with 200 mL of bisphenol A epoxy resin E-44 (including curing agent T31100 mL) and polyurethane resin (Covestro Desmophen® C1200), and coated on the metal surface with a coating thickness of 20 μm. After curing for 24 hours, the cyclic salt spray test was used for testing. The specific experimental conditions are shown in Table 1 below.
[0072]
[0073] After the test is completed, observe whether each paint film sample has bubbling or shedding to determine the anti-corrosion effect of the paint anti-corrosion materials prepared in Examples 1-3 and Comparative Examples 1-3 in the paint. The test results are shown in Table 2 below.
[0074]
[0075] From the results in Table 2, it can be seen that the paint anticorrosive materials prepared in Examples 1-3 have good corrosion resistance in epoxy resin and polyurethane resin.
[0076] After the paint waste is oxidized, the organic compounds in the system are further oxidized, forming a more stable and complex molecular structure in the system, which is beneficial to improving the corrosion resistance of the material; and the introduction of catechol groups using the carboxyl groups obtained after oxidation can improve the compatibility of the system with other materials, forming a more uniform system, thereby improving its corrosion resistance.
[0077] Now, the performance test of the paint anticorrosive materials prepared in Examples 1-3 and Comparative Examples 1-3 is performed. 10 g of the paint anticorrosive materials prepared in different groups are mixed with 200 mL of bisphenol A epoxy resin E-44 (including 100 mL of curing agent T31), and coated on the surface of metal substrates, glass substrates and wooden substrates with a coating thickness of 20 μm. After curing for 24 hours, the adhesion and hardness of the paint are tested. Among them, the adhesion of the paint film is measured according to the method in GB / T1720-1979, and the hardness of the paint film is tested according to the method in GB / T 6739-2022. The test results are shown in Table 3 below.
[0078]
[0079] From the results in Table 3, it can be seen that the paint anticorrosive materials prepared in Examples 1-3 show the best adhesion and hardness in the paint, and the adhesion on the surfaces of different substrates is improved, and the adhesion effect on the surface of the metal substrate is the best. From the results in the three comparative examples, it can be seen that the introduction of new catechol groups into paint waste can increase the degree of crosslinking inside the prepared paint system, thereby increasing the hardness of the paint surface. Since the catechol groups have good reactivity to a variety of substrates, the connection effect between the paint surface and the substrate is improved.
[0080] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0081] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for converting paint waste residue into paint anti-corrosion materials, characterized in that: The following steps are involved: S1. Collecting paint waste, drying at 50-80°C, dissolving the paint waste residue with a waste solvent, homogenizing and filtering, collecting the filtrate and the filtrate; grinding, crushing and sieving the filtrate after drying to obtain component A, and storing it for standby use; S2, add glacial acetic acid, sulfuric acid, metal oxide and oxidant to the filtrate obtained in step S1, stir evenly, raise the system temperature to 60-90°C, stir and react for 0.5-3 hours, then cool to room temperature, filter the system, let the filtrate stand and separate, collect the filtered material to obtain component B; collect the organic phase to obtain a waste system; The volume mass ratio of the filtrate to the glacial acetic acid, the sulfuric acid solution, the metal oxide and the oxidant is 300 mL: (50-80) mL: (10-20) mL: (5-10) g: (10-30) g; S3, mixing the waste system obtained in step S2 with dopamine hydrochloride, introducing catechol groups into the system, and obtaining a modified waste system; Wherein, the modified waste system is specifically prepared by the following steps: 2-morpholineethanesulfonic acid is added to the waste system to adjust the pH value of the system to 5.1, and then 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride are added to the system, and stirred for reaction for 5-10 hours under an inert atmosphere to obtain a modified waste system; the mass ratio of the waste system to dopamine hydrochloride is 400:(0.5-5.0); S4, removing water from the modified waste system, and finally mixing it with component A obtained in step S1 and component B obtained in step S2, stirring evenly and then mixing it with the reinforcing material in any ratio to obtain a paint anticorrosive material; Wherein, the reinforcing material is at least one of graphene, SiO2, amphoteric compounds, metal powder and zinc salt.
2. The method for converting paint waste residue into paint anti-corrosion materials according to claim 1, characterized in that: In step S1, the waste solvent is obtained by mixing alcohols, esters and aromatic hydrocarbons.
3. The method for converting paint waste residue into paint anti-corrosion materials according to claim 2, characterized in that: The ester is at least one of ethyl acetate and butyl butyrate, and the aromatic hydrocarbon is at least one of toluene and xylene.
4. The method for converting paint waste residue into paint anti-corrosion materials according to claim 2, characterized in that: The waste solvent is obtained by mixing ethanol, ethyl acetate and xylene in a mass ratio of (1-3): (0.1-2):
5.
5. The method for converting paint waste residue into paint anti-corrosion materials according to claim 1, characterized in that: In step S2, the sulfuric acid is a 40-70wt% sulfuric acid solution; the oxidant is at least one of potassium permanganate, hydrogen peroxide, hypochlorite, potassium dichromate, sodium periodate or nitric acid; and the metal oxide is at least one of chromium trioxide, cupric oxide and ferrous oxide.