Silicon carbide porous ceramic corrugated plate and preparation method and use thereof

By using alternating slurry and silicone sintering methods containing silicon powder and without silicon powder in porous media combustion technology, silicon carbide ceramic corrugated plates are formed, which solves the problem of insufficient high temperature resistance and thermal shock resistance, and achieves high efficiency Thermal shock and anti-oxidation properties.

CN118239794BActive Publication Date: 2024-11-29ZHONGKE ZHUOYI GREENE TECH (DONGGUAN) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410413918.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-11-29
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

The existing porous media combustion technology lacks high temperature resistance and insufficient thermal shock resistance, especially in high temperature environments, materials are prone to low strength and poor oxidation resistance.

Method used

Two slurries containing silicon powder and without silicon powder are alternately slurry, and a carbon layer and a silicon combination layer are formed by the first pyrolysis sintering, and an antioxidant layer is formed during the second silicon permeation sintering process to enhance the surface and interior. The combination of the silicon carbide ceramic corrugated plate improves the thermal shock resistance of the silicon carbide ceramic corrugated plate.

Benefits of technology

It significantly improves the thermal shock resistance and strength of silicon carbide porous ceramic corrugated plates, can maintain a strength of more than 95.3% at high temperatures, and the oxidation weight gain rate is less than 0.31% in simulated combustion environment, and has excellent oxidation resistance and avoids The problem of cracking at the bonding area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118239794B_ABST
    Figure CN118239794B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon carbide porous ceramic corrugated plate and a preparation method and use thereof, the preparation method comprising: a substrate is subjected to a first alternating slurry with a first bottom slurry and a second bottom slurry in sequence to obtain a first substrate; the first bottom slurry comprises silicon carbide powder, a high carbon yield resin, a curing agent and a solvent, and the first bottom slurry does not contain silicon powder; the second bottom slurry comprises silicon carbide powder, a first organic resin, silicon powder and a solvent; the first substrate is pressed and heated to be formed into a wavy piece, the wavy piece is subjected to a second alternating slurry with the first bottom slurry and the second bottom slurry in sequence to obtain a wavy piece carrying slurry; the wavy piece carrying slurry is subjected to a first pyrolysis sintering to obtain a precursor; the precursor is immersed in a surface slurry and subjected to a second siliconization sintering to obtain the silicon carbide ceramic corrugated plate. The present invention improves the strength, thermal shock resistance and oxidation resistance of silicon carbide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic corrugated plate preparation, and in particular to a silicon carbide porous ceramic corrugated plate and a preparation method and application thereof. Background Art

[0002] Porous media combustion is a method in which fuel and oxidant burn in the pores of porous media, and the heat transfer form is mainly high-temperature solid radiation. The gas generates vortices, splits and merges in the tiny cavities of the porous media material, and violent disturbances form countless small flames. The heat generated by the combustion is continuously transferred upstream and downstream through the thermal conductivity and radiation effects of the porous media. The temperature distribution in the entire combustion area is uniform, and there is no high temperature point. Compared with free flame combustion, porous media combustion has the advantages of high combustion rate, good stability, uniform heat separation, and no local high temperature; NO x The porous medium combustion technology solves the shortcomings of the traditional free flame combustion technology, such as uneven temperature distribution, serious pollutant emissions, high energy consumption, and large combustion space.

[0003] In view of the needs of high temperature resistance, thermal shock resistance and thermal shock resistance required for porous media combustion, it is very important to develop high temperature resistant and highly thermal shock resistant porous ceramics. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a silicon carbide porous ceramic corrugated plate and a preparation method and use thereof. The present invention significantly improves the thermal shock resistance of the silicon carbide porous ceramic corrugated plate by alternately hanging two slurries containing silicon powder and not containing silicon powder. At the same time, the surface slurry is used for the second siliconization sintering, and the internal siliconization reaction is carried out while the anti-oxidation layer is formed, so that the surface anti-oxidation layer and the internal silicon carbide are more firmly bonded and the thermal shock resistance is stronger.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a silicon carbide porous ceramic corrugated plate, the preparation method comprising:

[0007] (1) a substrate is subjected to a first alternating coating with a first bottom slurry and a second bottom slurry in sequence to obtain a first substrate; the first bottom slurry comprises silicon carbide powder, a high carbon yield resin, a curing agent and a solvent, and the first bottom slurry does not contain silicon powder; the second bottom slurry comprises silicon carbide powder, a first organic resin, silicon powder and a solvent;

[0008] (2) The first substrate is pressed and heated to be formed into a corrugated member, and the corrugated member is then subjected to a second alternating coating with a first bottom slurry and a second bottom slurry in sequence to obtain a corrugated member carrying slurry;

[0009] (3) The corrugated member carrying the slurry is subjected to a first pyrolysis and sintering to obtain a precursor;

[0010] (4) The precursor is immersed in a surface slurry and subjected to a second siliconization and sintering to obtain the silicon carbide ceramic corrugated plate.

[0011] It is worth mentioning that there are two main ways to sinter silicon carbide ceramics. One is to use a slurry containing silicon powder, pyrolyze it, and then directly perform siliconization and sintering to form silicon carbide ceramics; the other is to use a slurry without silicon powder and perform siliconization reaction in a silicon-containing environment to form silicon carbide ceramics. However, the first method using a slurry containing silicon powder is prone to voids during the production process, resulting in low silicon carbide strength; and the second method of silicon carbide production process is prone to internal carbon residues that fail to form silicon carbide because silicon is infiltrated from the external environment to the inside, and the thickness of the infiltration is limited. In view of the above situation, the present application creatively adopts alternating impregnation of a slurry containing silicon powder and a slurry without silicon powder, so that the first matrix formed by the two forms a C layer and a mixed layer of C and silicon respectively during the subsequent first pyrolysis sintering, wherein the first bottom slurry without silicon powder forms a carbon layer, and the second bottom slurry containing silicon powder forms a combined layer of carbon and silicon-containing substances; then after immersion in the surface slurry, a siliconizing reaction is carried out during the subsequent second siliconizing sintering process, wherein the carbon layer reacts with the silicon seeping from the combined layer of carbon and silicon-containing substances to form silicon carbide, and the combined layer of carbon and silicon-containing substances not only reacts itself to form silicon carbide, but also part of the silicon seeps into the carbon layer during the reaction, thereby forming a silicon carbide layer for the entire material; the design of this step can simultaneously have the advantages of external siliconizing and internal siliconizing reactions, and silicon carbide has excellent thermal shock resistance and high strength.

[0012] Furthermore, during the second siliconizing sintering process, the surface slurry gradually forms an anti-oxidation layer, that is, the anti-oxidation layer and the siliconizing reaction proceed simultaneously, which significantly improves the bonding strength between the surface anti-oxidation layer and silicon carbide, and the thermal shock resistance of the overall material is improved.

[0013] Preferably, the material of the substrate in step (1) includes organic resin.

[0014] The present invention has no special requirements for the organic resin, and any material that can be used for the substrate known to those skilled in the art can be used. Preferably, the substrate includes organic resin foam, organic resin woven organic mesh, or 3D printed organic resin porous plate.

[0015] Preferably, the mass ratio of silicon carbide powder, high carbon yield resin and curing agent in the first base slurry is 70-20:25-55:1-20, wherein the number of silicon carbide powder can be, for example, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25 or 20, the number of high carbon yield resin can be, for example, 25, 30, 35, 40, 45, 48, 50, 52 or 55, and the number of curing agent can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 13, 15, 18 or 20, etc.

[0016] The present invention has no restriction on the specific selection of high carbon yield resin and curing agent, and any material known to those skilled in the art for high carbon yield resin and curing agent can be used, and can also be adjusted according to actual conditions. High carbon yield resin refers to a resin with a residual carbon value greater than 35%, for example, it can be one of epoxy resin, phenolic resin, polyacrylic resin, polyvinyl butyral, furfural resin or phenol furfural resin, or a mixture of at least two thereof; the curing agent can be one of citric acid, p-toluenesulfonic acid, pentosine or oxalic acid, or a mixture of at least two thereof.

[0017] Preferably, the solid content of the first bottom layer slurry is 25-75wt%, for example, it can be 25wt%, 31wt%, 37wt%, 42wt%, 48wt%, 53wt%, 59wt%, 64wt%, 70wt% or 75wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0018] In the present application, the solid content and silicon carbide powder content in the first bottom layer slurry are set relatively low, and the high carbon yield resin content is higher, which is used to form silicon carbide with the silicon powder in the second bottom layer slurry, thereby improving the interaction between the first bottom layer slurry and the second bottom layer slurry, and improving the strength and thermal shock resistance of silicon carbide.

[0019] Preferably, the solvent of the first bottom layer slurry is an alcohol solvent.

[0020] The present invention has no limitation on the specific selection of the alcohol solvent of the first bottom layer slurry, and any material that can be used for alcohol solvents known to those skilled in the art can be used, and can also be adjusted according to actual conditions, such as ethanol, etc. Other solvents such as formaldehyde, etc. can also be used.

[0021] Preferably, the content of silicon powder in the second base slurry in step (1) is 0.1-0.5wt%, for example, it can be 0.1wt%, 0.12wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt% or 0.5wt%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0022] The silicon powder content in the second bottom layer slurry of the present invention is selected to be lower than the existing content, and is used to react with the residual carbon produced by the pyrolysis of the resin in the first bottom layer slurry to obtain silicon carbide, thereby improving the bonding force between the two layers and ensuring the bonding strength of silicon carbide. There is no need to remove excess silicon in the subsequent step, and the operation process is simpler.

[0023] Preferably, the silicon powder content in the second bottom layer slurry increases first and then decreases from the substrate surface outward.

[0024] The present invention preferably adopts a silicon powder distribution method in which the silicon powder content in the second bottom layer slurry first increases and then decreases, so that a product with a more uniform silicon carbide content in the overall coating can be better obtained in the subsequent siliconization reaction.

[0025] Preferably, from the surface of the substrate to the outside, the number of layers of the second bottom layer slurry is sequentially recorded as the 1st layer to the nth layer, where n is the total number of layers of the second bottom layer slurry, and the value range of n is a natural number from 2 to 100; and from the surface of the substrate to the outside, the silicon powder content of the second bottom layer slurry in the i-th layer to the n-th layer is less than the silicon powder content of the second bottom layer slurry in the 1st layer to the j-th layer, which is less than the silicon powder content of the second bottom layer slurry in the j+1-th layer to the i-1-th layer, where 1≤j≤i≤n.

[0026] Preferably, the mass ratio of silicon carbide powder, first organic resin, silicon powder and solvent in the second bottom layer slurry is (10-15): (6-7): (6-10): (60-80), wherein the proportion of silicon carbide powder can be, for example, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5 or 15, etc.; the proportion of the first organic resin can be, for example, 6 .0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9 or 7.0, etc.; the number of parts of silicon powder can be, for example, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5 or 10, etc.; the number of parts of the solvent can be, for example, 60, 61, 62, 63, 64, 65, 66, 67, 68, 68, 70, 72, 75, 78 or 80, etc.

[0027] The present invention has no limitation on the specific selection of the first organic resin in the second bottom layer slurry. Any organic resin material that can be used for the bottom layer slurry and is well known to those skilled in the art can be used. The material can also be adjusted according to actual conditions. The first organic resin can be, for example, one of epoxy resin, phenolic resin, polyacrylic resin, polyvinyl butyral, furfural resin or phenol furfural resin or a mixture of at least two of them.

[0028] Preferably, the solvent in the second bottom layer slurry comprises one or a mixture of at least two of castor oil, triolein, Tween 20 or organic bentonite.

[0029] The present invention has no limitation on the specific selection of the solvent, and any material that can be used as a solvent and is well known to those skilled in the art can be used, and can also be adjusted according to actual conditions, for example, it can be ethanol and / or formaldehyde.

[0030] Preferably, drying or spin-drying is performed after each slurrying.

[0031] Preferably, the number of the first alternating slurry coating is 1 to 2 alternating cycles.

[0032] Preferably, the second alternating slurry coating is performed until a slurry layer having a target thickness is obtained.

[0033] Preferably, the pressing in step (2) comprises: placing the first substrate in a mold or pressing with rollers.

[0034] Preferably, the heating and setting temperature is 150-250°C, for example, it can be 150°C, 162°C, 173°C, 184°C, 195°C, 206°C, 217°C, 228°C, 239°C or 250°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0035] Preferably, the ratio of the amplitude to the wavelength of the wavy member is (0.25-0.7):1, for example, it can be 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.65:1 or 0.7:1, etc., but is not limited to the listed values, and other values ​​not listed within this range are also applicable.

[0036] Preferably, the temperature of the first pyrolysis sintering in step (3) is 600-1000°C, for example, it can be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0037] Preferably, the temperature rise degree of the first pyrolysis and sintering includes: heating to a first temperature of 600-800°C at a heating rate of 4°C / min-5°C / min and keeping warm for 2-3 hours in the pyrolysis stage, and heating to a second temperature of 800-1000°C at a heating rate of 1-3°C / min and keeping warm for 4-5 hours in the sintering stage.

[0038] The temperature is raised to a first temperature of 600-800°C at a heating rate of 4°C / min-5°C / min and maintained for 2-3h. The temperature may be, for example, 4°C / min, 4.2°C / min, 4.3°C / min, 4.4°C / min, 4.5°C / min, 4.6°C / min, 4.7°C / min, 4.8°C / min, 4.9°C / min or 5°C / min, but is not limited to the values ​​listed. Other values ​​not listed in the range are also applicable. 600-800°C ℃, for example, it can be 600℃, 620℃, 630℃, 640℃, 650℃, 660℃, 680℃, 700℃, 720℃, 750℃, 760℃ or 800℃, but it is not limited to the listed values, and other values ​​not listed in this range are also applicable; 2-3h, for example, it can be 2h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h, but it is not limited to the listed values, and other values ​​not listed in this range are also applicable.

[0039] Then, the temperature is raised to a second temperature of 800-1000°C at a heating rate of 1-3°C / min and kept at this temperature for 4-5h. The heating rate of 1-3°C / min may be, for example, 1°C / min, 1.3°C / min, 1.5°C / min, 1.7°C / min, 1.9°C / min, 2.2°C / min, 2.4°C / min, 2.6°C / min, 2.8°C / min or 3°C / min, but is not limited to the values ​​listed. Other values ​​not listed in this range are also applicable. 800-1000°C, for example For example, it may be 800°C, 820°C, 830°C, 840°C, 850°C, 860°C, 880°C, 900°C, 920°C, 950°C, 960°C or 1000°C, but is not limited to the listed values, and other values ​​not listed in this range are equally applicable; 4 to 5h, for example, it may be 4h, 4.2h, 4.3h, 4.4h, 4.5h, 4.6h, 4.7h, 4.8h, 4.9h or 5h, but is not limited to the listed values, and other values ​​not listed in this range are equally applicable.

[0040] Preferably, the surface slurry in step (4) comprises REAl3C3, chromium oxide, a second resin and water, wherein RE represents a rare earth element, such as any one of Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu, or a combination of at least two thereof.

[0041] Preferably, the mass ratio of the surface slurry is (40-50): (10-30): (25-40), wherein the number of REAl3C3 is 40, 41, 42, 43, 44, 45, 48 or 50, etc.; the number of chromium oxide can be, for example, 10, 12, 15, 18, 20, 22, 25, 28 or 30, etc.; the number of the second resin can be, for example, 25, 28, 30, 32, 35, 38 or 40, etc.

[0042] Preferably, the second resin is a phenolic resin.

[0043] The present invention preferably uses phenolic resin, and the residual carbon produced by pyrolysis of the resin reacts with silicon to generate a certain amount of silicon carbide, thereby enhancing the bonding between the surface coating and the internal slurry, reducing the difference in thermal expansion coefficients, and preventing the surface layer from peeling off easily.

[0044] Preferably, the solid content of the surface slurry is 60-70wt%, for example, it can be 60wt%, 61.2wt%, 62.3wt%, 63.4wt%, 64.5wt%, 65.6wt%, 66.7wt%, 67.8wt%, 68.9wt% or 70wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0045] Preferably, the temperature of the second siliconizing sintering is 1300-1800°C, for example, it can be 1300°C, 1356°C, 1412°C, 1467°C, 1523°C, 1578°C, 1634°C, 1689°C, 1745°C or 1800°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0046] Preferably, the temperature rising degree of the second siliconizing sintering includes: heating to a third temperature of 1000-1100°C at a heating rate of 0.5°C / min-1.5°C / min, then heating to a fourth temperature of 1300-1500°C at a heating rate of 2-3°C / min and keeping warm for 1-3h, then heating to 1600-1800°C at a heating rate of 4-6°C / min and keeping warm for 2-2.5h, and cooling to room temperature with the furnace.

[0047] Wherein, the temperature is increased to the third temperature of 1000-1100°C at a heating rate of 0.5°C / min-1.5°C / min, 0.5-1.5°C / min, for example, 0.5°C / min, 0.7°C / min, 0.8°C / min, 0.9°C / min, 1°C / min, 1.1°C / min, 1.2°C / min, 1.3°C / min, 1.4°C / min or 1.5°C / min, etc., but not limited to the listed values, and other values ​​not listed in the range are also applicable; 1000-1100°C, for example, 1000°C, 1012°C, 1023°C, 1034°C, 1045°C, 1056°C, 1067°C, 1078°C, 1089°C or 1100°C, etc., but not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0048] Then, the temperature is raised to a fourth temperature of 1300-1500° C. at a heating rate of 2-3° C. / min and kept at this temperature for 1-3 hours. The heating rate may be 2° C. / min, 2.2° C. / min, 2.3° C. / min, 2.4° C. / min, 2.5° C. / min, 2.6° C. / min, 2.7° C. / min, 2.8° C. / min, 2.9° C. / min or 3° C. / min, but is not limited to the values ​​listed. Other values ​​not listed in this range are also applicable. 1300-1500° C., For example, it may be 1300°C, 1320°C, 1340°C, 1360°C, 1380°C, 1410°C, 1430°C, 1450°C, 1470°C or 1500°C, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; 1 to 3h, for example, it may be 1h, 1.3h, 1.5h, 1.7h, 1.9h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0049] Then, the temperature is raised to 1600-1800°C at a heating rate of 4-6°C / min and kept at that temperature for 2-2.5h, 4-6°C / min, for example, 4°C / min, 4.3°C / min, 4.5°C / min, 4.7°C / min, 4.9°C / min, 5.2°C / min, 5.4°C / min, 5.6°C / min, 5.8°C / min or 6°C / min, but is not limited to the values ​​listed, and other values ​​not listed in the range are also applicable; 1600 ~1800℃, for example, it can be 1600℃, 1620℃, 1645℃, 1660℃, 1680℃, 1715℃, 1730℃, 1750℃, 1770℃ or 1800℃, but it is not limited to the listed values, and other values ​​not listed in the range are equally applicable; 2~2.5h, for example, it can be 2h, 2.1h, 2.2h, 2.3h, 2.4h or 2.5h, but it is not limited to the listed values, and other values ​​not listed in the range are equally applicable.

[0050] During the second siliconizing sintering process, the formation of the anti-oxidation layer and the internal siliconizing reaction are carried out simultaneously, which makes the surface anti-oxidation layer and the internal silicon carbide more firmly bonded and has stronger thermal shock resistance. In addition, the surface slurry contains REAl3C3, which reacts at about 900-1300℃ after hydrolysis and forms Re3Al5O with chromium oxide. 12 / Al2O3 / Cr2O3 composite oxide helps sintering densification and improves the material's antioxidant properties.

[0051] Preferably, the preparation method further comprises: stacking at least two silicon carbide ceramic corrugated plates of step (4) to form a silicon carbide porous ceramic corrugated plate.

[0052] The present application directly stacks silicon carbide ceramic corrugated plates to form silicon carbide porous ceramic corrugated plates without using adhesives, thereby avoiding the problem of cracking of the bonding parts during high-temperature use, resulting in the silicon carbide porous ceramic corrugated plates being unusable.

[0053] Preferably, the angle between the fluid channel formed by stacking between the individual silicon carbide porous ceramic corrugated plates and the fluid flow direction is 15 to 85°, for example, it can be 15°, 16°, 17°, 18°, 20°, 25°, 30°, 35°, 40°, 45°, 50°, 60°, 70°, 80° or 85°, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0054] When the silicon carbide porous ceramic corrugated plate of the present invention is used for combustion purposes, low flow resistance is required, preferably around 20-45°; when used for filling purposes, distillation requires increasing the heat exchange time and the disorder of gas-liquid flow, preferably around 30-60°.

[0055] As a preferred technical solution of the first aspect of the present invention, the method for preparing the silicon carbide porous ceramic corrugated plate comprises the following steps:

[0056] (1') the substrate is alternately coated with a first bottom slurry and a second bottom slurry in sequence, and each coating is followed by drying or spin drying to obtain a first substrate;

[0057] Specifically, the first bottom layer slurry includes silicon carbide powder, high carbon yield resin, curing agent and solvent, and the first bottom layer slurry does not contain silicon powder; the mass ratio of silicon carbide powder, high carbon yield resin and curing agent in the first bottom layer slurry is (70-20): (25-55): (1-20); the solid content in the first bottom layer slurry is 25-75wt%; the solvent of the first bottom layer slurry is an alcohol solvent;

[0058] The second bottom layer slurry comprises silicon carbide powder, a first organic resin, silicon powder and a solvent; the content of silicon powder in the second bottom layer slurry is 0.1-0.5wt%; the mass ratio of silicon carbide powder, the first organic resin, silicon powder and the solvent in the second bottom layer slurry is (10-15): (6-7): (6-10): (60-80); the solvent is an alcohol solvent; from the surface of the substrate to the outside, the number of layers of the second bottom layer slurry is recorded as the 1st layer to the nth layer, wherein n is the total number of layers of the second bottom layer slurry, and the value range of n is a natural number of 2-100; and from the surface of the substrate to the outside, the silicon powder content of the second bottom layer slurry in the i-th layer to the n-th layer is less than the silicon powder content of the second bottom layer slurry in the 1st layer to the j-th layer < the silicon powder content of the second bottom layer slurry in the j+1th layer to the i-1th layer, wherein 1≤j≤i≤n;

[0059] (2') The first substrate is placed in a mold or rolled and heated at 150-250° C. to be formed into a wavy piece, wherein the ratio of the amplitude to the wavelength of the wavy piece is (0.25-0.7):1;

[0060] (3') The wavy member is subjected to a first pyrolysis sintering, wherein the first pyrolysis sintering temperature rise degree includes: heating to a first temperature of 600-800°C at a heating rate of 4°C / min-5°C / min and keeping the temperature for 2-3 hours, and then heating to a first temperature of 800-1000°C at a heating rate of 1-3°C / min and keeping the temperature for 4-5 hours to obtain a precursor;

[0061] (4') the precursor is immersed in a surface slurry, wherein the mass ratio of the surface slurry is (40-50) of REAl3C3, chromium oxide and the second resin: (10-30) : (25-40), the solid content of the surface slurry is 60-70wt%, and the precursor is subjected to a second siliconization sintering, wherein the temperature rise degree of the second siliconization sintering includes: heating to a first temperature of 1000-1100°C at a heating rate of 0.5°C / min-1.5°C / min, then heating to a first temperature of 1300-1500°C at a heating rate of 2-3°C / min and keeping the temperature for 1-3h, then heating to 1600-1800°C at a heating rate of 4-6°C / min and keeping the temperature for 2-2.5h, removing unreacted silicon, and cooling to room temperature with the furnace to obtain the silicon carbide ceramic corrugated plate;

[0062] (5') stacking at least two silicon carbide ceramic corrugated plates of step (4'), wherein the angle between the fluid channel formed by stacking between the individual silicon carbide porous ceramic corrugated plates and the fluid flow direction is 15 to 85 degrees, to form a silicon carbide porous ceramic corrugated plate.

[0063] In a second aspect, the present invention provides a silicon carbide porous ceramic corrugated plate, wherein the silicon carbide porous ceramic corrugated plate is prepared by the method for preparing the silicon carbide porous ceramic corrugated plate described in the first aspect.

[0064] The silicon carbide porous ceramic corrugated plate provided in the second aspect of the present invention has excellent mechanical strength and strong thermal shock resistance.

[0065] In a third aspect, the present invention provides a use of the silicon carbide porous ceramic corrugated plate described in the first aspect in a burner medium and / or a distillation filler.

[0066] The silicon carbide porous ceramic corrugated plate provided by the present invention has the advantages of strong acid and alkali resistance and low flow resistance when used as distillation filler, and has the advantages of high emissivity, excellent thermal conductivity and strong thermal shock resistance when used as burner medium. Compared with the prior art, the present invention has at least the following beneficial effects:

[0067] (1) The preparation method of the silicon carbide porous ceramic corrugated plate provided by the present invention adopts two slurries containing silicon powder and not containing silicon powder for alternate slurrying, which improves the strength of silicon carbide and can ensure uniform distribution of components within the thickness range of silicon carbide; the strength retention rate of the silicon carbide porous ceramic corrugated plate with a volume fraction of 40% obtained by the present invention before and after thermal shock is more than 95.3%, and there is no crack after more than 60 thermal shock tests at 1300°C, and the thermal shock resistance is excellent;

[0068] (2) The method for preparing the silicon carbide porous ceramic corrugated plate provided by the present invention simultaneously performs the siliconization reaction and the formation of the surface anti-oxidation layer during the second siliconization sintering process, thereby improving the bonding strength between the surface anti-oxidation layer and the silicon carbide. Compared with the prior art of first completely preparing the silicon carbide and then preparing the surface oxidation layer, it saves one step of the sintering process, greatly reduces energy consumption, and has lower costs;

[0069] (3) The silicon carbide porous ceramic corrugated plate provided by the present invention preferably adds REAl3C3 to the surface slurry to form Re3Al5O 12 / Al2O3 / Cr2O3 composite oxide has high antioxidant performance, and its oxidation weight gain rate in a simulated combustion environment is preferably within 0.31%. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 It is a schematic diagram of the precursor obtained in step (3') of Example 1 of the present invention.

[0071] Figure 2 It is a schematic diagram of the silicon carbide ceramic corrugated plate obtained in step (4') of Example 1 of the present invention.

[0072] Figure 3 It is a schematic diagram of the silicon carbide porous ceramic corrugated plate obtained in step (5') of Example 1 of the present invention. DETAILED DESCRIPTION

[0073] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0074] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0075] Example 1

[0076] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate, the preparation method comprising the following steps:

[0077] (1') A 3D printed organic resin porous plate (specifically made of PP-R Sinopec Yangzi C180 brand 5000S polyethylene) is sequentially subjected to a first base slurry and a second base slurry for a first alternating slurry coating, and each slurry coating is followed by drying or spin drying, and after two alternating slurry coatings, a first substrate is obtained;

[0078] Specifically, the first bottom layer slurry includes silicon carbide powder, high carbon yield resin (specific material is E-44 (6101) epoxy resin), curing agent (specific material is citric acid) and ethanol, and the first bottom layer slurry does not contain silicon powder; the mass ratio of silicon carbide powder, high carbon yield resin and curing agent in the first bottom layer slurry is 60:25:15; the solid content in the first bottom layer slurry is 50wt%;

[0079] The second bottom layer slurry includes silicon carbide powder, a first organic resin (specifically, phenolic resin DER331A), silicon powder and a solvent (ethanol); the content of silicon powder in the second bottom layer slurry is 0.2wt%; the mass ratio of silicon carbide powder, the first organic resin, silicon powder and the solvent in the second bottom layer slurry is 10:7:8:75;

[0080] (2') The first substrate is placed in a mold or rolled and heated at 200° C. to be formed into a wavy piece, wherein the ratio of the amplitude to the wavelength of the wavy piece is 0.5:1; the wavy piece is then subjected to a second alternating slurry coating with the first bottom slurry and the second bottom slurry in sequence, the second alternating slurry coating is performed 10 times, and a wavy piece carrying slurry is obtained;

[0081] The content of silicon powder in the second bottom slurry in the 1st to 5th second alternating slurrying is 0.4wt%, and the content of silicon powder in the second bottom slurry in the 6th to 10th second alternating slurrying is 0.1wt%;

[0082] (3') The wavy member carrying the slurry is subjected to a first pyrolysis sintering, wherein the first pyrolysis sintering temperature rise degree includes: heating to a first temperature of 800°C at a heating rate of 4.5°C / min and keeping the temperature for 3 hours, and then heating to a second temperature of 1000°C at a heating rate of 3°C / min and keeping the temperature for 4.5 hours to obtain a precursor, see Figure 1 ;

[0083] (4') The precursor is immersed in a surface slurry, wherein the mass ratio of the surface slurry is 50:20:30 among REAl3C3, chromium oxide and the second resin (MF1 type phenolic resin), and the solid content of the surface slurry is 65wt%. After a silicon block is arranged on the surface of the precursor, a second siliconization sintering is performed. The temperature rise degree of the second siliconization sintering includes: heating to a third temperature of 1050°C at a heating rate of 1.0°C / min, then heating to a fourth temperature of 1400°C at a heating rate of 2.5°C / min and keeping the temperature for 2h, then heating to 1700°C at a heating rate of 5°C / min and keeping the temperature for 2.3h, removing unreacted silicon, and cooling to room temperature with the furnace to obtain the silicon carbide ceramic corrugated plate with a thickness of 5mm, see Figure 2 ;

[0084] (5') stacking at least two silicon carbide ceramic corrugated plates of step (4'), wherein the angle between the fluid channel formed by stacking between the single silicon carbide porous ceramic corrugated plates and the fluid flow direction is 45°, to form a silicon carbide porous ceramic corrugated plate, see Figure 3 .

[0085] Example 2

[0086] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate, the preparation method comprising the following steps:

[0087] (1') The foam foamed by organic resin (specifically, the material is HTK-2030 polyurethane) is subjected to a first alternating slurry with a first bottom slurry and a second bottom slurry in sequence, and each time the slurry is applied, the foam is dried or spun off, and the first substrate is obtained after two alternating slurries;

[0088] Specifically, the first bottom layer slurry includes silicon carbide powder, high carbon yield resin (specifically, E-44 (6101) epoxy resin), curing agent (specifically, oxalic acid) and ethanol, and the first bottom layer slurry does not contain silicon powder; the mass ratio of silicon carbide powder, high carbon yield resin and curing agent in the first bottom layer slurry is 70:25:5; the solid content in the first bottom layer slurry is 25wt%;

[0089] The second bottom layer slurry includes silicon carbide powder, a first organic resin (specifically, phenolic resin DER331A), silicon powder and a solvent (formaldehyde); the content of silicon powder in the second bottom layer slurry is 0.3wt%; the mass ratio of silicon carbide powder, the first organic resin, silicon powder and the solvent in the second bottom layer slurry is 15:6:10:69;

[0090] (2') The first substrate is placed in a mold or rolled and heated at 150° C. to be formed into a wavy piece, wherein the ratio of the amplitude to the wavelength of the wavy piece is 0.25:1; the wavy piece is then subjected to a second alternating slurry coating with the first bottom slurry and the second bottom slurry in sequence, wherein the second alternating slurry coating is performed 15 times, thereby obtaining a wavy piece carrying slurry;

[0091] Among them, the content of silicon powder in the second bottom slurry in the 1st to 3rd second alternating slurry is 0.35wt%, the content of silicon powder in the second bottom slurry in the 4th to 10th second alternating slurry is 0.5wt%, and the content of silicon powder in the second bottom slurry in the 11th to 15th second alternating slurry is 0.2wt%;

[0092] (3') The corrugated member carrying the slurry is subjected to a first pyrolysis sintering, wherein the first pyrolysis sintering temperature rise degree includes: heating to a first temperature of 600° C. at a heating rate of 4° C. / min and keeping the temperature for 2 hours, and then heating to a second temperature of 900° C. at a heating rate of 1° C. / min and keeping the temperature for 5 hours, to obtain a precursor;

[0093] (4') The precursor is immersed in a surface slurry, wherein the mass ratio of the surface slurry is 40:25:35 among REAl3C3, chromium oxide and the second resin (MF1 type phenolic resin), the solid content of the surface slurry is 70wt%, and a silicon block is arranged on the surface of the precursor and then subjected to a second siliconization sintering, wherein the temperature rise degree of the second siliconization sintering includes: heating to a third temperature of 1100°C at a heating rate of 1.5°C / min, then heating to a fourth temperature of 1500°C at a heating rate of 3°C / min and keeping the temperature for 1h, then heating to 1800°C at a heating rate of 4°C / min and keeping the temperature for 2.5h, removing unreacted silicon, and cooling to room temperature with the furnace to obtain the silicon carbide ceramic corrugated plate with a thickness of 7mm;

[0094] (5') stacking at least two silicon carbide ceramic corrugated plates of step (4'), wherein the angle between the fluid channel formed by stacking between the individual silicon carbide porous ceramic corrugated plates and the fluid flow direction is 30°, to form a silicon carbide porous ceramic corrugated plate.

[0095] Example 3

[0096] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate, the preparation method comprising the following steps:

[0097] (1') an organic mesh woven with an organic resin (specifically made of PS-polystyrene 685D) is subjected to a first alternating slurry coating with a first bottom slurry and a second bottom slurry in sequence, and each slurry coating is followed by drying or spin drying. After two alternating slurry coatings, a first substrate is obtained;

[0098] Specifically, the first bottom layer slurry includes silicon carbide powder, high carbon yield resin (specific material is E-44 (6101) epoxy resin), curing agent (specific material is p-toluenesulfonic acid) and ethanol, and the first bottom layer slurry does not contain silicon powder; the mass ratio of silicon carbide powder, high carbon yield resin and curing agent in the first bottom layer slurry is 50:30:20; the solid content of the first bottom layer slurry is 70wt%;

[0099] The second bottom layer slurry includes silicon carbide powder, a first organic resin (specifically, phenolic resin DER331A), silicon powder and a solvent (ethanol); the content of silicon powder in the second bottom layer slurry is 0.15wt%; the mass ratio of silicon carbide powder, the first organic resin, silicon powder and the solvent in the second bottom layer slurry is 10:7:6:77;

[0100] (2') The first substrate is placed in a mold or rolled and heated at 250° C. to be formed into a wavy piece, wherein the ratio of the amplitude to the wavelength of the wavy piece is 0.7:1; the wavy piece is then subjected to a second alternating slurry coating with the first bottom slurry and the second bottom slurry in sequence, wherein the second alternating slurry coating is performed 20 times, thereby obtaining a wavy piece carrying slurry;

[0101] Among them, the content of silicon powder in the second bottom slurry in the 1st to 5th second alternating slurry is 0.20wt%, the content of silicon powder in the second bottom slurry in the 6th to 10th second alternating slurry is 0.25wt%, the content of silicon powder in the second bottom slurry in the 11th to 15th second alternating slurry is 0.45wt%, and the content of silicon powder in the second bottom slurry in the 15th to 20th second alternating slurry is 0.10wt%;

[0102] (3') The corrugated member carrying the slurry is subjected to a first pyrolysis sintering, wherein the first pyrolysis sintering temperature rise degree includes: heating to a first temperature of 700° C. at a heating rate of 5° C. / min and keeping the temperature for 3 hours, and then heating to a second temperature of 800° C. at a heating rate of 3° C. / min and keeping the temperature for 4 hours, to obtain a precursor;

[0103] (4') The precursor is immersed in a surface slurry, wherein the mass ratio of the surface slurry is 45:15:40 among REAl3C3, chromium oxide and the second resin (MF2 phenolic resin), the solid content of the surface slurry is 60wt%, and a silicon block is arranged on the surface of the precursor and then subjected to a second siliconization sintering, wherein the temperature rise degree of the second siliconization sintering includes: heating to a third temperature of 1000°C at a heating rate of 0.5°C / min, then heating to a fourth temperature of 1300°C at a heating rate of 2.5°C / min and keeping the temperature for 3h, then heating to 1700°C at a heating rate of 6°C / min and keeping the temperature for 2h, removing unreacted silicon, and cooling to room temperature with the furnace to obtain the silicon carbide ceramic corrugated plate with a thickness of 7.5mm;

[0104] (5') stacking at least two silicon carbide ceramic corrugated plates of step (4'), wherein the angle between the fluid channels formed by stacking between the individual silicon carbide porous ceramic corrugated plates and the fluid flow direction is 60°, to form a silicon carbide porous ceramic corrugated plate.

[0105] Example 4

[0106] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the surface slurry in step (4') does not contain REAl3C3, and the details are not described again.

[0107] Example 5

[0108] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the surface slurry in step (4') does not contain chromium oxide, and the details are not described again.

[0109] Example 6

[0110] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the MF1 phenolic resin in the surface slurry in step (4') is replaced by NeoPacE106 polyurethane resin, and the details are not repeated here.

[0111] Example 7

[0112] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the content of silicon powder in the second bottom layer slurry is 3% and the content of solvent is increased accordingly, and will not be repeated here.

[0113] Example 8

[0114] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the content of silicon powder in the second bottom layer slurry is 15% and the content of solvent is reduced accordingly, and will not be repeated here.

[0115] Example 9

[0116] The present embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that in step (5'), at least two silicon carbide ceramic corrugated plates in step (4') are bonded with a binder to form a silicon carbide porous ceramic corrugated plate, and thus will not be described in detail.

[0117] Example 10

[0118] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the final temperature of the first pyrolysis sintering in step (3') is 1500°C, and will not be described in detail here.

[0119] Specifically, the first pyrolysis sintering includes: heating to a first temperature of 800°C at a heating rate of 4.5°C / min and keeping it for 3 hours, then heating to a second temperature of 1000°C at a heating rate of 3°C / min and keeping it for 4.5 hours, and then heating to 1500°C at a heating rate of 5°C / min and keeping it for 2.3 hours.

[0120] Embodiment 11

[0121] This embodiment provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Embodiment 1 except that the content of silicon powder in the second bottom slurry in step (2') is 0.2 wt %, and will not be described again.

[0122] Comparative Example 1

[0123] This comparative example provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as Example 1 except that the first bottom layer slurry contains 0.4wt% silicon powder and the proportions of other substances remain unchanged, and will not be repeated here.

[0124] Comparative Example 2

[0125] This comparative example provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as that of Example 1, except that the second bottom layer slurry does not contain silicon powder, and will not be described in detail here.

[0126] Comparative Example 3

[0127] This comparative example provides a method for preparing a silicon carbide porous ceramic corrugated plate. The preparation method is the same as Example 1 except that the surface slurry is not impregnated at all, and the details are not repeated here.

[0128] The compressive strength of the sample was tested using a universal pressure testing machine. Figure 3 The surface shown is the test stress surface, the loading rate is 0.5mm / min, and the test ends when the load drops to 40% of the maximum load. The residual compressive strength of the sample after the thermal shock test is measured using a universal pressure testing machine with the same parameters, and the strength retention rate of the same group of samples before and after the thermal shock is calculated. The compressive strength of the sample is obtained by averaging 6 samples.

[0129] The combustion method was used to test the antioxidant properties. In a combustion environment simulated, the above-mentioned ceramic samples (size: 800mm×30mm×20mm) were placed in a high temperature of 1400℃, carbon dioxide, and water vapor environment for 150h. SiC first reacted with water vapor to generate SiO2, and the oxide layer SiO2 continued to react with water vapor to generate Si(OH)4. The oxidation rate of SiC was calculated based on the mass change (oxidation weight gain) before and after the combustion test of the sample; (SiC will gain weight when oxidized to SiO2, and the weight of the generated Si(OH)4 will decrease after volatilization. In actual tests, oxidation and volatilization are dynamic processes that exist simultaneously. The test result is weight gain but reduced density, and the appearance of micropores. The simplest method is to measure the oxidation weight gain).

[0130] The thermal shock resistance of the sample was tested by the water quenching method. The sample was placed in a heating furnace at 1300°C for 20 minutes, and then quickly placed in running water at 25°C. After the sample was cooled, it was taken out and dried. The above process was repeated N times to observe whether there were cracks. The test results of the above embodiments and comparative examples are shown in Table 1.

[0131] Table 1

[0132]

[0133]

[0134] In Table 1, "40% volume fraction" means 60% porosity.

[0135] From Table 1, we can see the following points:

[0136] (1) It can be seen from Examples 1 to 3 that the silicon carbide porous ceramic corrugated plate provided by the present invention has an excellent strength retention rate, which is more than 95.3% before and after thermal shock, and the oxidation weight gain rate in a simulated combustion environment is within 0.31%, and the anti-oxidation performance is excellent. After more than 60 times of thermal shock test at 1300°C, there is no crack, and the thermal shock resistance is excellent;

[0137] (2) It can be seen from Example 1, Examples 4 to 6, and Comparative Example 3 that when the components in the surface slurry are not within the preferred composition range, the oxidation weight gain of Examples 4 to 6 increases, and the antioxidant performance of the silicon carbide porous ceramic corrugated plate decreases. The oxidation weight gain in Comparative Example 3 is even increased to 1.5%, which shows that the present invention can significantly improve the antioxidant performance of the product by optimizing and rationally designing the components in the surface slurry;

[0138] (3) Combining Example 1, Example 7-8, Example 11 and Comparative Example 2, it can be seen that the silicon powder content in the second bottom layer slurry in Example 11 is within the preferred range, but the silicon powder content of each coating is the same, and its strength retention rate is lower than that in Example 1, and the oxidation weight gain increases to 0.31%, indicating that the present invention can better ensure the strength and antioxidant properties of the product by preferably setting the silicon powder content in the second bottom layer slurry to increase and then decrease from the substrate surface to the outside; the silicon powder content in Examples 7-8 is high, and its strength retention rate decreases to 92.7% and 93.0%, respectively, and the oxidation weight gain is 0. The weight is as high as 0.41% and 0.33% respectively. In Example 8, due to the serious excess of silicon powder content, the thermal shock resistance is significantly reduced. After 60 thermal shock tests, local fine cracks are generated; in Comparative Example 2, no silicon powder is added, resulting in the final second siliconizing sintering being similar to conventional siliconizing sintering, the strength retention rate is reduced to 93.3%, and the oxidation weight gain is increased. This shows that the selection of silicon powder content in the second bottom layer slurry of the present invention and the preferred design of the change of silicon powder content with the change of the number of slurry layers can further improve the thermal shock resistance, oxidation resistance and strength retention rate of the silicon carbide porous ceramic corrugated plate;

[0139] (4) It can be seen from Example 1 and Example 9 that in Example 9, a binder is used to bond silicon carbide ceramic corrugated plates to form a porous ceramic corrugated plate, and obvious cracks appear at the bonding point during the thermal shock test. This shows that the present invention can form a porous ceramic corrugated plate by only stacking silicon carbide ceramic corrugated plates, which can leave enough expansion space for thermal expansion and contraction, thereby avoiding cracking during the thermal shock process;

[0140] (5) It can be seen from Example 1 and Example 10 that the final temperature of the first pyrolysis sintering in Example 1 is controlled at 1000°C. Compared with the final temperature of the first pyrolysis sintering in Example 10 being controlled at 1500°C, the sintering of the precursor is achieved in the first pyrolysis sintering process, which is isolated from the sintering process of the subsequent anti-oxidation layer, resulting in a decrease in the bonding degree of the subsequent anti-oxidation layer and a local surface layer peeling phenomenon in the thermal shock test. This shows that the present invention can significantly improve the bonding degree by controlling the temperature of the first pyrolysis sintering within 1000°C, thereby co-sintering the precursor slurry and the subsequent anti-oxidation layer, thereby improving the thermal shock resistance of the overall material;

[0141] (6) It can be seen from Example 1 and Comparative Example 1 that the first bottom slurry in Example 1 does not contain silicon powder. Compared with the case where the first bottom slurry in Comparative Example 1 contains silicon powder, the thermal shock resistance, oxidation resistance and strength retention rate of the silicon carbide porous ceramic corrugated plate in Example 1 are higher. This is because the first bottom slurry in Comparative Example 1 contains silicon powder, and silicon reacts with carbon to form silicon carbide, and the molecular size changes to form voids. When all slurries contain silicon, the overall strength and hardness of silicon carbide are significantly reduced. This shows that the present invention improves the strength and thermal shock resistance of silicon carbide by only arranging silicon powder in the second bottom slurry.

[0142] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a silicon carbide porous ceramic corrugated plate, characterized in that: The preparation method comprises: (1) A substrate is subjected to a first alternating coating with a first bottom slurry and a second bottom slurry in sequence to obtain a first substrate; the first bottom slurry comprises silicon carbide powder, a high carbon yield resin, a curing agent and a solvent, and the first bottom slurry does not contain silicon powder; the second bottom slurry comprises silicon carbide powder, a first organic resin, silicon powder and a solvent; the content of silicon powder in the second bottom slurry ranges from 0.1 to 0.5 wt%; from the surface of the substrate to the outside, the content of silicon powder in the second bottom slurry first increases and then decreases; The material of the substrate in step (1) includes organic resin; The mass ratio of silicon carbide powder, high carbon yield resin and curing agent in the first bottom layer slurry is 70-20:25-55:1-20; The solid content of the first bottom layer slurry is 25-75wt%; The mass ratio of silicon carbide powder, first organic resin, silicon powder and solvent in the second bottom layer slurry is (10-15): (6-7): (6-10): (60-80); (2) The first substrate is pressed and heated to be formed into a corrugated member, and the corrugated member is then subjected to a second alternating coating with a first bottom slurry and a second bottom slurry in sequence to obtain a corrugated member carrying slurry; (3) The corrugated member carrying the slurry is subjected to a first pyrolysis and sintering to obtain a precursor; (4) The precursor is immersed in a surface slurry and subjected to a second siliconization and sintering to obtain a silicon carbide ceramic corrugated plate; The surface slurry in step (4) comprises REAl3C3, chromium oxide, a second resin and water, wherein RE represents a rare earth element; The mass ratio of the surface slurry is that the mass ratio of REAl3C3, chromium oxide and the second resin is (40-50): (10-30): (25-40); The solid content of the surface slurry is 60-70wt%.

2. The preparation method according to claim 1, characterized in that: The matrix includes foam formed by organic resin foaming, organic mesh woven by organic resin, or a 3D-printed organic resin porous plate.

3. The preparation method according to claim 1, characterized in that: The solvent of the first bottom layer slurry is an alcohol solvent.

4. The preparation method according to claim 1, characterized in that: From the surface of the substrate to the outside, the number of layers of the second bottom layer slurry is recorded as the 1st layer to the nth layer, where n is the total number of layers of the second bottom layer slurry, and the value range of n is a natural number from 2 to 100; and from the surface of the substrate to the outside, the silicon powder content of the second bottom layer slurry in the i-th layer to the n-th layer is less than the silicon powder content of the second bottom layer slurry in the 1st layer to the j-th layer, which is less than the silicon powder content of the second bottom layer slurry in the j+1-th layer to the i-1-th layer, where 1<j≤i≤n.

5. The preparation method according to claim 1, characterized in that: The solvent in the second bottom layer slurry includes one of castor oil, triolein or Tween 20 or a mixture of at least two of them.

6. The preparation method according to claim 1, characterized in that: After each slurrying, drying or spin-drying is performed.

7. The preparation method according to claim 1, characterized in that: The number of the first alternating slurry coating is 1 to 2 alternating cycles.

8. The preparation method according to claim 1, characterized in that: The second alternating slurry coating is performed until a slurry layer having a target thickness is obtained.

9. The preparation method according to claim 1, characterized in that: The pressing in step (2) includes: placing the first substrate in a mold or pressing with rollers.

10. The preparation method according to claim 1, characterized in that: The temperature of the heating and setting is 150-250°C.

11. The preparation method according to claim 1, characterized in that: The ratio of the amplitude to the wavelength of the wavy member is (0.25-0.7):

1.

12. The preparation method according to claim 1, characterized in that: Step (3) The temperature of the first pyrolysis sintering is 600-1000°C.

13. The preparation method according to claim 1, characterized in that: The temperature rise degree of the first pyrolysis and sintering includes: heating to a first temperature of 600-800°C at a heating rate of 4°C / min-5°C / min and keeping warm for 2-3 hours in the pyrolysis stage, and heating to a second temperature of 800-1000°C at a heating rate of 1-3°C / min and keeping warm for 4-5 hours in the sintering stage.

14. The preparation method according to claim 1, characterized in that: The temperature of the second siliconizing sintering is 1300-1800°C.

15. The preparation method according to claim 1, characterized in that: The temperature rise degree of the second siliconizing sintering includes: heating to a third temperature of 1000~1100°C at a heating rate of 0.5°C / min~1.5°C / min, then heating to a fourth temperature of 1300~1500°C at a heating rate of 2~3°C / min and keeping warm for 1~3h, then heating to 1600~1800°C at a heating rate of 4~6°C / min and keeping warm for 2~2.5h, and cooling to room temperature with the furnace.

16. The preparation method according to claim 1, characterized in that: The preparation method further comprises: stacking at least two silicon carbide ceramic corrugated plates of step (4) to form a silicon carbide porous ceramic corrugated plate.

17. The preparation method according to claim 16, characterized in that: The angle between the fluid channel formed by stacking the individual silicon carbide porous ceramic corrugated plates and the fluid flow direction is 15-85 degrees.

18. A silicon carbide porous ceramic corrugated plate, characterized in that: The silicon carbide porous ceramic corrugated plate is prepared by the preparation method of the silicon carbide porous ceramic corrugated plate according to any one of claims 1 to 17.

19. Use of the silicon carbide porous ceramic corrugated plate according to claim 18 in burner media and / or distillation filler.

Citation Information

Patent Citations

  • Silicon carbide foamed ceramics corrugated structured packing and preparation method and applications thereof

    CN102218293A

  • High-strength porous silicon carbide ceramic material and preparation method thereof

    CN114195547A

  • Silicon carbide porous ceramic as well as preparation method and application thereof

    CN117003580A