Green high-viscosity and toughness asphalt modifier, modified asphalt and preparation method and concrete
Through the secondary melt blended extrusion method and the peeling of layered nanoclay materials, the problems of insufficient viscosity of asphalt modifiers and easy agglomeration of nanomaterials are solved, and low-cost and high-performance asphalt modifiers and asphalt concrete are realized. Suitable for extremely heavy, extremely heavy and heavy traffic, extending the service life of asphalt pavement.
Patent Information
- Application Number
- CN202410304640.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-18
AI Technical Summary
Existing asphalt modifiers have insufficient viscosity in extremely heavy, extra heavy and heavy-duty traffic applications, nanomaterials are prone to agglomeration, poor compatibility, high stability and cost, making it difficult to meet the needs of high-performance asphalt.
The green high viscosity tough asphalt modifier is prepared by secondary melt blending and extrusion method. Through the peeling of layered nanoclay materials and the optimized formulation of waste rubber and plastic, the dispersion of nanoclay materials and the phase of waste rubber and plastic materials is improved. Capacity, reduce costs.
It realizes low-cost, green, low-carbon, high viscosity and high toughness asphalt modifiers and asphalt concrete, improves the stability and comprehensive performance of asphalt, is suitable for extremely heavy, heavy-duty traffic, and extends the asphalt pavement. Service life.
Smart Images

Figure CN118240392B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of asphalt concrete for road engineering, and specifically to a green high-viscosity and toughness asphalt modifier, modified asphalt, a preparation method and concrete, and especially to a green high-viscosity and toughness asphalt modifier, modified asphalt, a preparation method and concrete suitable for extremely heavy, extra heavy and heavy load traffic. Background Art
[0002] As one of the main raw materials for asphalt pavement, petroleum asphalt is a mixture of some extremely complex high molecular hydrocarbons and non-metallic (oxygen, sulfur, nitrogen) derivatives of these hydrocarbons formed by the long-term exposure of petroleum to geophysical factors under natural environmental conditions. However, due to the widespread and serious phenomenon of highway overloading and heavy loading, the road surface, especially the asphalt surface layer, is also subjected to the repeated effects of severe climatic environments such as large temperature differences, freezing rain and snow, and strong ultraviolet rays, which causes frequent road cracking, rutting and other diseases. According to current standards, the design life of highway asphalt pavement is 15 years, but through research, it is found that more than 70% of highways need major or medium repairs after about 10 years of use, resulting in huge consumption of resources and energy, serious environmental pollution and damage, and hindering the sustainable development of highways. The performance of traditional matrix asphalt is difficult to meet the needs of the growing traffic volume. Therefore, the research and development of high-performance asphalt has also attracted more and more attention from road workers, and improving the matrix asphalt with asphalt modifiers to obtain high-performance asphalt is currently the most important way.
[0003] SBS (styrene-butadiene-styrene triblock copolymer) is a commonly used asphalt modifier. SBS modifier can significantly improve the weather resistance, load resistance, low-temperature flexibility, high-temperature fluidity and other properties of asphalt. It can greatly improve the performance of asphalt and extend the service life of asphalt. Therefore, it has been widely used in the existing technology.
[0004] For example, Chinese patent document CN108034270A discloses a modified asphalt and a preparation method thereof. The modified asphalt provided is prepared from the following raw materials in parts by weight: 100-120 parts of asphalt, 6-20 parts of modifier, 3-9 parts of compatibilizer, 0.15-0.25 parts of sulfur, 0.4-0.6 parts of non-amine anti-stripping agent and 0.2-0.4 parts of coupling agent; the modifier includes styrene-butadiene-styrene block copolymer (SBS), rubber and polyurethane. A high-viscosity modified asphalt for permeable asphalt paving system is prepared by combining high-speed shearing and colloid milling. The modified asphalt provided by the scheme can simultaneously meet the following requirements: elastic recovery ≥ 98% at 25°C, dynamic viscosity ≥ 500,000 Pa·s at 60°C, composite shear modulus ≥ 10kPa at 60°C, critical temperature ≥ 94°C of G* / Sinδ ≥ 2.2kPa.
[0005] Chinese patent document CN115304925A discloses a low melting point, fast-dissolving, high-viscosity asphalt modifier and a preparation method thereof, wherein the asphalt modifier comprises the following raw materials in weight: 8-15 parts of magnesium-aluminum dihydroxy composite metal hydroxide; 12-14 parts of antioxidant; 10-15 parts of heavy aromatic oil; 0.4-2 parts of silane coupling agent a151; 40-60 parts of SBS rubber powder; 0.01-0.05 parts of graphene; 20-25 parts of aromatic extracted oil; 3-10 parts of tetraethyl silicate, and 12-21 parts of modifier.
[0006] The above two existing technical solutions use SBS and rubber as the main components of the modifier. On the one hand, since the production of SBS modifier involves petrochemical raw materials, it is unsustainable and costly; and the SBS modifier has a C=C double bond, which is very easy to age, which can easily lead to a sharp decline in performance. On the other hand, rubber-modified asphalt has problems such as excessive viscosity at high temperatures, making it difficult to ensure construction and workability. In addition, the porosity of the permeable asphalt paving system is extremely large (about 15%-25%). If the high-viscosity asphalt prepared by the solution disclosed in CN108034270A is used in the permeable asphalt paving system, the high-viscosity asphalt is easy to contact with air, which will reduce the service performance of the high-viscosity permeable asphalt pavement. The solution disclosed in CN115304925A also adds graphene material as a modifying material. Graphene material is a very expensive material, which will further increase the cost of the high-viscosity modifier, thereby affecting its practical application.
[0007] In order to overcome the problems existing in the above-mentioned SBS / rubber asphalt modifier, the prior art has proposed to use nanomaterials and waste rubber powder for modification, which can solve the problem of high cost of SBS / rubber modification.
[0008] For example, Chinese patent document CN107227031A discloses a nano-composite asphalt modifier and its preparation method, wherein the modifier includes the following components by weight: 3-5 parts of modified nano-material; 30-50 parts of thermoplastic styrene elastomer; 30-40 parts of recycled rubber powder; 20-40 parts of recycled polyethylene material; 1-2 parts of vulcanizing agent; maleic anhydride grafted PE is 1.5%-3% of the amount of the recycled polyethylene material. This invention scheme increases the lipophilicity of the nano-material and improves the dispersibility of the nano-material in asphalt by first surface treating the nano-material. The incorporation of the nano-material into the modifier can further improve the high and low temperature stability of the modified asphalt added with the modifier of the present invention.
[0009] According to the requirements specially marked in the "Technical Specification for Design and Construction of Drained Asphalt Pavement" JTG / T 3350-03-2020, the dynamic viscosity of high-viscosity modified asphalt should be appropriately increased for extremely heavy, extra heavy and heavy-load traffic, preferably above 20wPa·s. The most important indicator of high-viscosity asphalt is the dynamic viscosity at 60°C, that is, for extremely heavy, extra heavy and heavy-load traffic, the dynamic viscosity at 60°C should be above 20wPa·s. The nanomaterial and waste rubber powder composite modifier and modified asphalt provided by the above-mentioned prior art CN107227031A, with reference to its disclosed performance data, the dynamic viscosity at 60°C of its best embodiment (Example 3) is only 15.7wPa·s, which is far from meeting the viscosity requirements of extremely heavy, extra heavy and heavy-load traffic, thereby limiting the application of asphalt. In addition, although the composite modification of nanomaterials and waste rubber powder can solve the problem of high cost of SBS / rubber modification, due to the high specific surface energy and surface area of nanoparticles, they are easy to agglomerate with waste rubber powder during the mixing process, thereby affecting the dispersion and uniformity of the material, thereby affecting the stability and other properties of the material.
[0010] Therefore, it is urgent to develop a high-viscosity, high-performance asphalt modifier, modified asphalt and its preparation method and asphalt concrete with low cost, good stability, simple preparation and wide application range, which is especially suitable for extremely heavy, extra heavy and heavy load transportation. Summary of the invention
[0011] The technical problem to be solved by the present invention is to provide a green high-viscosity and tough asphalt modifier, modified asphalt, preparation method and concrete. Its purpose is to optimize the formula and preparation process of the modifier, firstly use environmentally friendly raw materials, and creatively propose to use a secondary melt blending extrusion method to prepare a green high-viscosity and tough asphalt modifier, so as to better realize the stripping of layered nanoclay materials, solve the problem that nanoclay materials are difficult to disperse in waste rubber and plastic-based materials, and finally realize the research and development of low-cost, green, low-carbon, high-viscosity and tough modified asphalt and asphalt concrete.
[0012] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0013] In a first aspect, the present invention provides a green high-viscosity and high-toughness asphalt modifier, which comprises the following raw material components in parts by weight:
[0014] 70-232 parts of waste rubber and plastic mixture;
[0015] 4 to 10 parts of nano clay material;
[0016] 15-30 parts of compatibilizer;
[0017] The composite material is prepared by a secondary melt blending extrusion method.
[0018] Furthermore, the waste rubber and plastic mixture consists of waste rubber and waste plastic, and the mass ratio of waste rubber to waste plastic is 1:0.8-1.5.
[0019] Furthermore, the waste rubber is waste rubber powder, the particle size of which is 40-120 meshes, and the rubber hydrocarbon content is greater than 50%.
[0020] Furthermore, the waste plastics are waste polyethylene particles or waste polypropylene particles, and the particle size thereof is 10 to 15 meshes, and the particles are required to be uniform and full.
[0021] Furthermore, the nano-clay material includes at least one of nano-organic montmorillonite, nano-rectorite, and nano-vermiculite.
[0022] Furthermore, the compatibilizer is aromatic oil, and the aromatic content thereof is greater than 80%.
[0023] Furthermore, the method for preparing the asphalt modifier by the secondary melt blending extrusion method specifically comprises the following steps:
[0024] (1) Preparing a masterbatch by melt blending and extrusion: weighing nano-clay material, waste rubber and plastic mixture, and compatibilizer according to a mass ratio of 1:2-4:1-2, mixing at high speed, and extruding and granulating to obtain a masterbatch;
[0025] (2) Preparing an asphalt modifier by secondary melt blending and extrusion: the waste rubber and plastic mixture, the masterbatch prepared in step (1), and the compatibilizer are uniformly mixed at a mass ratio of 5-9:1-5:1-3 at high speed, and then extruded and granulated for a secondary time to obtain the asphalt modifier.
[0026] Furthermore, the high-speed mixing of step (1) is carried out in a high-speed mixer. Preferably, the speed of the high-speed mixer is controlled at 300 to 450 r / min, and the mixing time is controlled at 15 to 20 minutes.
[0027] Furthermore, the high-speed mixing in step (2) is carried out in a high-speed mixer. Preferably, the speed of the high-speed mixer is controlled at 300 to 450 r / min, and the mixing time is controlled at 15 to 20 minutes.
[0028] Furthermore, the extrusion process of step (1) is carried out by a twin-screw extruder. A twin-screw extruder can achieve high yield, high quality and high efficiency in the preparation of composite materials, so the present invention selects a twin-screw extruder.
[0029] Preferably, the barrel of the twin-screw extruder in step (1) comprises a feed section, a discharge section and at least one intermediate section, the temperature of the feed section and the discharge section is controlled at 170°C, the temperature of the intermediate section is controlled at 175°C, and the screw speed is 100-180r / min.
[0030] Preferably, the barrel of the twin-screw extruder comprises a feed section, a discharge section and 7 intermediate sections, and the temperatures of each section are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, and 170°C from the feed end to the discharge end.
[0031] Furthermore, the material after extrusion in step (1) is cooled in a water tank and then pulled to a granulator for primary granulation, and the rotation speed of the granulator is 200 to 400 r / min.
[0032] Furthermore, the extrusion process of step (2) is carried out by a twin-screw extruder. A twin-screw extruder can achieve high yield, high quality and high efficiency in the preparation of composite materials, so the present invention selects a twin-screw extruder.
[0033] Preferably, the barrel of the twin-screw extruder in step (2) comprises a feed section, a discharge section and at least one intermediate section, the temperature of the feed section and the discharge section is controlled at 170°C, the temperature of the intermediate section is controlled at 175°C, and the screw speed is 100-180r / min.
[0034] Preferably, the barrel of the twin-screw extruder comprises a feed section, a discharge section and 7 intermediate sections, and the temperatures of each section are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, and 170°C from the feed end to the discharge end.
[0035] Furthermore, the extruded material in step (2) is cooled in a water tank and then pulled to a granulator for secondary granulation, and the rotation speed of the granulator is 200 to 400 r / min.
[0036] Furthermore, the particle size of the masterbatch obtained in step (1) is controlled to be 10 to 15 meshes.
[0037] Furthermore, the particle size of the asphalt modifier obtained in step (2) is controlled to be 10 to 15 meshes.
[0038] In a second aspect, the present invention provides a green high-viscosity and high-toughness modified asphalt, comprising a base asphalt and the above-mentioned green high-viscosity and high-toughness asphalt modifier.
[0039] Furthermore, the mass ratio of the green high-viscosity and toughness asphalt modifier to the base asphalt is 15-20:80-85.
[0040] In a third aspect, the present invention provides a method for preparing the above-mentioned green high-viscosity and toughness modified asphalt.
[0041] Furthermore, the preparation method specifically comprises the following steps:
[0042] (1) The base asphalt is heated until it melts.
[0043] (2) Take out the melted base asphalt, add the green high-viscosity and toughness asphalt modifier into the base asphalt according to a preset ratio, control the temperature at 175-180° C., and stir preliminarily. In this step, low-speed preliminarily stirring is adopted, such as manual stirring.
[0044] (3) After preliminary stirring, the mixed material is subjected to high-speed shearing for 20 to 30 minutes, and the temperature is controlled at 175 to 180°C.
[0045] (4) Afterwards, the mixture is dispersed by stirring at a speed of 300 to 500 r / min, the dispersion time is controlled within 10 to 15 minutes, and the temperature is controlled within 175 to 180°C.
[0046] (5) Finally, the material obtained in step (4) is kept warm at 175-185° C. and sealed for development for 60-70 minutes to obtain the modified asphalt.
[0047] In the above preparation method: the purpose of step (3) is to grind the asphalt modifier, and the high-speed shear process is generally carried out using a high-speed shearing instrument; the purpose of step (4) is to further disperse the ground asphalt modifier in the matrix asphalt, and the high-speed stirring and dispersing process is generally carried out in a high-speed agitator; the purpose of step (5) is to allow the asphalt modifier to be fully developed in the matrix asphalt and form a stable spatial network structure with the matrix asphalt.
[0048] Furthermore, in step (1), the base asphalt is heated at 135°C to 140°C for 30 to 40 minutes until it melts.
[0049] Furthermore, the high-speed shear rate in step (2) is 4500-6000 r / min.
[0050] In a fourth aspect, the present invention further provides an asphalt concrete, comprising the green high-viscosity and toughness modified asphalt mentioned above or the green high-viscosity and toughness modified asphalt obtained by the above method, and mineral material; the green high-viscosity and toughness modified asphalt accounts for 5% to 6% of the weight of the mineral material.
[0051] Furthermore, the mineral material includes aggregate and mineral powder, and the porosity of the mineral material is controlled at 3-6%.
[0052] The present invention also provides a method for preparing the above-mentioned asphalt concrete, which specifically comprises the following steps:
[0053] (1) Weigh green high-viscosity and tough modified asphalt in proportion, and prepare aggregate and mineral powder according to the mineral gradation requirements (such as the mineral gradation of AC-13 dense graded asphalt mixture shown in Table 1);
[0054] (2) heating the green high-viscosity and toughness modified asphalt at 175° C. to 185° C. for 30 to 40 minutes until it melts, and heating the aggregate for 4 to 8 hours for standby use;
[0055] (3) The aggregate and green high-viscosity and tough modified asphalt in step (2) are placed at 175° C. to 185° C. and stirred for 90 to 120 seconds; then the prepared mineral powder is added and the mixture is stirred for another 90 to 120 seconds at 175° C. to 185° C. to obtain asphalt concrete.
[0056] Table 1 AC-13 dense graded asphalt mixture mineral aggregate gradation
[0057] Screen size (mm) 16 13.2 9.5 4.75 2.36 1.18 0.6 0.3 0.15 0.075 Upper limit of gradation 100 100 85 68 50 38 28 20 15 8 Lower limit of gradation 100 90 68 38 24 15 10 7 5 4 Median gradation 100 95 76.5 53 37 26.5 19 13.5 10 6 Pass rate (%) 100 95 74 48.5 34 23.5 15 11 8.5 6
[0058] The present invention has the following beneficial effects:
[0059] 1. The present invention provides an asphalt modifier and modified asphalt and asphalt concrete by optimizing the formula and preparation process of the asphalt modifier, which has the characteristics of low cost, green and low carbon, high viscosity and high toughness.
[0060] 2. The present invention creatively proposes to adopt a secondary melt blending extrusion method to prepare the asphalt modifier and modified asphalt and concrete, which can better realize the stripping of layered nanoclay materials, solve the problem that nanoclay materials are difficult to disperse in waste rubber and plastic-based materials, and at the same time improve the compatibility between waste rubber and plastic materials and asphalt through the nano effect of nanoclay materials, thereby improving the comprehensive performance of asphalt and its concrete.
[0061] Since nanomaterial particles have high specific surface energy and surface area, the problem of nanomaterial particles easily agglomerating when mixed with waste rubber and plastic mixtures is solved during the mixing process. The present invention first melt-blended the waste rubber and plastic mixture with nanoclay materials and compatibilizers to make it easier for macromolecules to be inserted between the lamellae of layered silicate, which plays a role in stretching the distance between nanoclay layers. The nanoclay materials are initially dispersed, and a masterbatch containing a high content of nanoclay (content of 7.7% to 25%) is prepared by melt-blending and extruding. Then, the waste rubber and plastic mixture, the compatibilizer and the prepared masterbatch are directly blended, and a second melt-blending and extrusion dispersion is performed to further increase the dispersion of the nanoclay material.
[0062] 3. The waste rubber and plastic mixtures used in the raw materials of the present invention are all environmentally friendly materials, which can reduce material costs, while realizing the resource and high-value utilization of waste rubber and plastics, and can realize the research and development of low-cost, green and low-carbon modified asphalt, which is crucial for the transportation industry to achieve the "dual carbon" goal.
[0063] 4. The nanoclay material in the asphalt modifier of the present invention has a layered structure. Using the nanoclay material as an auxiliary dispersion stabilizer can balance the density difference between the waste rubber and plastic material and the matrix asphalt, improve the dispersibility and uniformity of the material, and improve the stability of the modified asphalt. And due to the layered structure of the nanoclay material, the waste rubber and plastic base molecules and the asphalt molecules can be embedded in the layered nanoclay channels to form a stable three-dimensional spatial network structure, thereby greatly improving the comprehensive performance of the asphalt.
[0064] 5. The asphalt modifier, modified asphalt and asphalt concrete provided by the present invention have the characteristics of high viscosity and high toughness. The key indicator of asphalt modifier is melt mass flow rate (190℃, 2.16kg)>10g / 10min; the key indicator of modified asphalt is rotational viscosity at 150℃ is less than 3Pa·s, 48h softening point difference is less than 0.8℃, softening point is greater than 100℃, 5℃ elongation is greater than 50cm, high temperature classification temperature is above 100℃, low temperature classification temperature is -24℃; 60℃ dynamic viscosity is greater than 500,000 Pa·s; the key indicator of asphalt concrete is rutting factor at 60℃ is greater than 6000 times / mm, and low temperature bending failure strain is greater than 3000με. It is suitable for the technical requirements of extremely heavy, extra heavy and heavy load transportation. Therefore, the asphalt modifier, modified asphalt and asphalt concrete provided by the present invention, while ensuring excellent construction and workability, also have excellent storage stability, high and low temperature performance, and can be used for drainage noise pavement, ultra-thin overlays, bridge deck pavements, airport overlays and other paving layers that have strict requirements on binders, and have a wide range of applications.
[0065] In summary, the asphalt modifier, modified asphalt and asphalt concrete provided by the present invention have the characteristics of low cost, green and low carbon, good stability, wide application range, high viscosity and high toughness, high comprehensive performance, etc., and the preparation process is simple and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 This is a microstructure diagram of the modified asphalt provided in Example 1 of the present invention.
[0067] Figure 2 This is a microstructure diagram of the modified asphalt provided in Example 2 of the present invention.
[0068] Figure 3 This is a microstructure diagram of the modified asphalt provided in Example 3 of the present invention.
[0069] Figure 4This is a microstructure diagram of the modified asphalt provided in Example 4 of the present invention.
[0070] Figure 5 The microstructure diagram of the modified asphalt provided for Comparative Example 1.
[0071] Figure 6 The microstructure diagram of the modified asphalt provided for Comparative Example 2. DETAILED DESCRIPTION
[0072] As used herein:
[0073] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0074] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0075] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0076] In these examples, parts and percentages are by mass unless otherwise indicated.
[0077] "Parts by mass" refers to the basic unit of measurement for the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0078] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0079] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Preferred embodiments of the present invention are provided in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0080] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing the specific embodiments and are not intended to limit the present invention. In the embodiments, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0081] Embodiment 1:
[0082] 1. This embodiment first provides a green high-viscosity modifier and a preparation method thereof, wherein: the modifier includes the following raw material components in parts by weight: 232 parts of a waste rubber and plastic mixture, specifically 129 parts of waste rubber powder with a particle size of 60 mesh (rubber hydrocarbon content > 50%), 103 parts of waste polyethylene with a particle size of 10 mesh; 4 parts of nano-organic montmorillonite; 28 parts of aromatic oil (aromatic content greater than 80%).
[0083] The preparation method comprises the following steps:
[0084] (1) One-step melt blending and extrusion to prepare masterbatch:
[0085] First, nano-organic montmorillonite, waste rubber and plastic mixture and aromatic oil were weighed and evenly mixed in a high-speed mixer in a ratio of 1:4:1. The speed of the high-speed mixer was controlled at 450 r / min and the mixing time was controlled at 15 minutes.
[0086] Then it is extruded through a twin-screw extruder, cooled in a water tank, and then pulled to a granulator for granulation to obtain a masterbatch. The extruder barrel includes a feed section, a discharge section and 7 intermediate sections. The temperature of each section from the feed end to the discharge end is 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, the screw speed is 120r / min, and the pelletizer speed is 200 / min; the masterbatch particle size is controlled to be 10-15 mesh.
[0087] (2) Preparation of asphalt modifier by secondary melt blending and extrusion:
[0088] First, the waste rubber and plastic mixture, the masterbatch prepared in step (1), and the aromatic oil are uniformly mixed in a high-speed mixer in a ratio of 9:1:1. The speed of the high-speed mixer is controlled at 450 r / min and the mixing time is controlled at 15 minutes.
[0089] Then, the asphalt modifier is prepared by extruding with a twin-screw extruder, cooling in a water tank, and then being pulled to a granulator for secondary granulation. The extruder barrel includes a feed section, a discharge section, and 7 intermediate sections. The temperatures of each section from the feed end to the discharge end are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, respectively. The screw speed is 120r / min, the pelletizer speed is 200r / min, and the particle size of the green high-viscosity and tough asphalt modifier is controlled at 10-15 meshes.
[0090] 2. This embodiment also provides a green high-viscosity and toughness modified asphalt and a preparation method thereof. The modified asphalt includes the following raw material components in parts by weight: 85 parts of 70# base asphalt and 15 parts of the green high-viscosity and toughness asphalt modifier prepared in the first part of this embodiment.
[0091] The preparation method comprises the following steps:
[0092] (1) heating the base asphalt in an oven at 135°C for 40 minutes;
[0093] (2) Take out the melted base asphalt and place it on an electromagnetic heating device, add the green high-viscosity and toughness asphalt modifier into the base asphalt, stir it manually for 15 minutes, and control the temperature at 180°C;
[0094] (3) After preliminary manual stirring, the modified asphalt was subjected to high-speed shearing at a rate of 4500 r / min for 30 minutes using a high-speed shearing instrument, and the temperature was controlled at 180°C;
[0095] (4) using a high-speed agitator to further disperse the modified asphalt after high-speed shearing, the dispersion time is controlled at 15 minutes, the speed is controlled at 300 r / min, and the temperature is controlled at 180° C.;
[0096] (5) The prepared modified asphalt is placed in a closed oven for development for 70 minutes at a temperature of 180° C. to obtain the green high-viscosity and tough modified asphalt.
[0097] 3. This embodiment also provides a method for preparing green high-viscosity and high-toughness asphalt concrete. The preparation method comprises the following steps:
[0098] (1) Weigh the following raw material components in parts by weight: 5 parts of the green high-viscosity and toughness asphalt prepared in the second part of this embodiment, 94 parts of aggregate, and 6 parts of mineral powder; the aggregate and mineral powder are configured according to the grading of the AC-13 dense-graded asphalt mixture mineral material shown in Table 1, the porosity is controlled at 3-6%, and the sieve size of the mineral powder is less than 0.075 mm.
[0099] (2) heating the green high-viscosity and toughness modified asphalt at 175° C. to 185° C. for 30 to 40 minutes until it melts, and heating the aggregate for more than 4 hours for later use;
[0100] (3) The aggregate and green high-viscosity and tough modified asphalt in step (2) are placed at 175° C. to 185° C. and stirred for 90 to 120 seconds; then the prepared mineral powder is added and the mixture is stirred for another 90 to 120 seconds at 175° C. to 185° C. to obtain asphalt concrete.
[0101] Embodiment 2:
[0102] 1. This embodiment first provides a green high-viscosity and toughness asphalt modifier and a preparation method thereof, wherein: the modifier includes the following raw material components in parts by weight: 112 parts of a waste rubber and plastic mixture, specifically 62 parts of waste rubber powder with a particle size of 100 mesh (rubber hydrocarbon content > 50%), 50 parts of waste polypropylene with a particle size of 10 mesh; 4 parts of nanorectorite; 16 parts of aromatic oil (aromatic content greater than 80%).
[0103] The preparation method comprises the following steps:
[0104] (1) One-step melt blending and extrusion to prepare masterbatch:
[0105] First, nanorectorite, waste rubber and plastic mixture and aromatic oil were weighed and evenly mixed in a high-speed mixer in a ratio of 1:4:1. The speed of the high-speed mixer was controlled at 450 r / min and the mixing time was controlled at 15 minutes.
[0106] Then it is extruded through a twin-screw extruder, cooled in a water tank, and then pulled to a granulator for granulation to obtain a masterbatch. The extruder barrel includes a feed section, a discharge section and 7 intermediate sections. The temperature of each section from the feed end to the discharge end is 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, the screw speed is 120r / min, and the pelletizer speed is 200 / min; the masterbatch particle size is controlled to be 10-15 mesh.
[0107] (2) Preparation of asphalt modifier by secondary melt blending and extrusion:
[0108] First, the waste rubber and plastic mixture, the masterbatch prepared in step (1), and the aromatic oil are uniformly mixed in a high-speed mixer in a ratio of 8:2:1. The speed of the high-speed mixer is controlled at 450 r / min and the mixing time is controlled at 15 minutes.
[0109] Then, the asphalt modifier is prepared by extruding with a twin-screw extruder, cooling in a water tank, and then being pulled to a granulator for secondary granulation. The extruder barrel includes a feed section, a discharge section, and 7 intermediate sections. The temperatures of each section from the feed end to the discharge end are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, respectively. The screw speed is 120r / min, the pelletizer speed is 200r / min, and the particle size of the green high-viscosity and tough asphalt modifier is controlled at 10-15 meshes.
[0110] 2. This embodiment also provides a green high-viscosity and toughness modified asphalt and a preparation method thereof. The modified asphalt includes the following raw material components in parts by weight: 85 parts of 70# base asphalt and 15 parts of the green high-viscosity and toughness asphalt modifier prepared in the first part of this embodiment.
[0111] The preparation method comprises the following steps:
[0112] (1) heating the base asphalt in an oven at 135°C for 40 minutes;
[0113] (2) Take out the melted base asphalt and place it on an electromagnetic heating device, add the green high-viscosity and toughness asphalt modifier into the base asphalt, stir it manually for 15 minutes, and control the temperature at 180°C;
[0114] (3) After preliminary manual stirring, the modified asphalt was subjected to high-speed shearing at a rate of 4500 r / min for 30 minutes using a high-speed shearing instrument, and the temperature was controlled at 180°C;
[0115] (4) using a high-speed agitator to further disperse the modified asphalt after high-speed shearing, the dispersion time is controlled at 15 minutes, the speed is controlled at 300 r / min, and the temperature is controlled at 180° C.;
[0116] (5) The prepared modified asphalt is placed in a closed oven for development for 70 minutes at a temperature of 180° C. to obtain the green high-viscosity and tough modified asphalt.
[0117] 3. This embodiment also provides a method for preparing green high-viscosity and tough asphalt concrete. The asphalt concrete includes the following raw material components by weight: 5 parts of green high-viscosity and tough asphalt prepared in the second part of this embodiment, 94 parts of aggregate, and 6 parts of mineral powder; the aggregate and mineral powder are configured according to the AC-13 dense-graded asphalt mixture mineral grading shown in Table 1, the porosity is controlled at 3-6%, and the sieve size of the mineral powder is less than 0.075 mm. The specific preparation method refers to Example 1.
[0118] Example 3
[0119] 1. This embodiment first provides a green high-viscosity and toughness asphalt modifier and a preparation method thereof, wherein: the modifier includes the following raw material components in parts by weight: 90 parts of a waste rubber and plastic mixture, specifically 50 parts of waste rubber powder with a particle size of 120 mesh (rubber hydrocarbon content > 50%), 40 parts of waste polypropylene with a particle size of 10 mesh; 5 parts of nano vermiculite; 15 parts of aromatic oil (aromatic content greater than 80%).
[0120] The preparation method comprises the following steps:
[0121] (1) One-step melt blending and extrusion to prepare masterbatch:
[0122] First, nano-vermiculite, waste rubber and plastic mixture and aromatic oil were weighed and mixed evenly in a high-speed mixer in a ratio of 1:4:1. The speed of the high-speed mixer was controlled at 450 r / min and the mixing time was controlled at 15 minutes.
[0123] Then it is extruded through a twin-screw extruder, cooled in a water tank, and then pulled to a granulator for granulation to obtain a masterbatch. The extruder barrel includes a feed section, a discharge section and 7 intermediate sections. The temperature of each section from the feed end to the discharge end is 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, the screw speed is 120r / min, the pelletizer speed is 200 / min, and the masterbatch particle size is controlled to be 10-15 mesh.
[0124] (2) Preparation of asphalt modifier by secondary melt blending and extrusion:
[0125] First, the waste rubber and plastic mixture, the masterbatch prepared in step (1), and the aromatic oil are uniformly mixed in a high-speed mixer in a ratio of 7:3:1, and the speed of the high-speed mixer is controlled at 450 r / min for 15 to 20 minutes;
[0126] Then, the asphalt modifier is prepared by extruding with a twin-screw extruder, cooling in a water tank, and then being pulled to a granulator for secondary granulation. The extruder barrel includes a feed section, a discharge section, and 7 intermediate sections. The temperatures of each section from the feed end to the discharge end are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, respectively. The screw speed is 120r / min, the pelletizer speed is 200r / min, and the particle size of the green high-viscosity and tough asphalt modifier is controlled at 10-15 meshes.
[0127] 2. This embodiment also provides a green high-viscosity and toughness modified asphalt and a preparation method thereof. The modified asphalt includes the following raw material components in parts by weight: 85 parts of 70# base asphalt and 15 parts of the green high-viscosity and toughness asphalt modifier prepared in the first part of this embodiment.
[0128] The preparation method comprises the following steps:
[0129] (1) heating the base asphalt in an oven at 135°C for 40 minutes;
[0130] (2) Take out the melted base asphalt and place it on an electromagnetic heating device, add the green high-viscosity and toughness asphalt modifier into the base asphalt, stir it manually for 15 minutes, and control the temperature at 180°C;
[0131] (3) After preliminary manual stirring, the modified asphalt was subjected to high-speed shearing at a rate of 4500 r / min for 30 minutes using a high-speed shearing instrument, and the temperature was controlled at 180°C;
[0132] (4) using a high-speed agitator to further disperse the modified asphalt after high-speed shearing, the dispersion time is controlled at 15 minutes, the speed is controlled at 300 r / min, and the temperature is controlled at 180° C.;
[0133] (5) The prepared modified asphalt is placed in a closed oven for development for 70 minutes at a temperature of 180° C. to obtain the green high-viscosity and tough modified asphalt.
[0134] 3. This embodiment also provides a method for preparing green high-viscosity and high-toughness asphalt concrete. The asphalt concrete comprises the following raw material components by weight: 5 parts of the green high-viscosity and high-toughness modified asphalt prepared in the second part of this embodiment, 94 parts of aggregate, and 6 parts of mineral powder; the aggregate and mineral powder are configured according to the AC-13 dense-graded asphalt mixture mineral grading shown in Table 1, the void ratio is controlled at 3-6%, and the sieve size of the mineral powder is less than 0.075 mm.
[0135] The specific preparation method is shown in Example 1.
[0136] Example 4
[0137] 1. This embodiment first provides a green high-viscosity modifier and a preparation method thereof, wherein: the modifier includes the following raw material components in parts by weight: 70 parts of a waste rubber and plastic mixture, specifically 28 parts of waste rubber powder with a particle size of 120 mesh (rubber hydrocarbon content>50%), 42 parts of waste polypropylene with a particle size of 10 mesh (mass ratio 1:1.5); 10 parts of nanorectorite; 50 parts of aromatic oil (aromatic content greater than 80%).
[0138] The preparation method comprises the following steps:
[0139] (1) One-step melt blending and extrusion to prepare masterbatch:
[0140] First, weigh nano-organic montmorillonite, waste rubber and plastic mixture and aromatic oil, and mix them evenly in a high-speed mixer in a ratio of 1:2:2. The speed of the high-speed mixer is controlled at 300 r / min, and the time is controlled at 15 to 20 minutes.
[0141] Then it is extruded through a twin-screw extruder, cooled in a water tank, and then pulled to a granulator for granulation to obtain a masterbatch. The extruder barrel includes a feed section, a discharge section and 7 intermediate sections. The temperature of each section from the feed end to the discharge end is 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, the screw speed is 180r / min, the pelletizer speed is 400 / min, and the masterbatch particle size is controlled to be 10-15 mesh.
[0142] (2) Preparation of asphalt modifier by secondary melt blending and extrusion:
[0143] First, the waste rubber and plastic mixture, the masterbatch prepared in step (1), and the aromatic oil are uniformly mixed in a high-speed mixer in a ratio of 5:5:3, the speed of the high-speed mixer is controlled at 300 r / min, and the mixing time is controlled at 15 to 20 minutes;
[0144] Then, after extrusion through a twin-screw extruder, the mixture is cooled in a water tank and then pulled to a granulator for secondary granulation to obtain the green high-viscosity and tough asphalt modifier. The extruder barrel includes a feed section, a discharge section and 7 intermediate sections, and the temperatures of each section from the feed end to the discharge end are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, respectively. The screw speed is 180r / min, the pelletizer speed is 400r / min, and the particle size of the green high-viscosity and tough asphalt modifier is controlled at 10-15 meshes.
[0145] Second, this embodiment also provides a green high-viscosity and toughness modified asphalt and a preparation method thereof, wherein: the modified asphalt comprises the following raw material components in parts by weight: 80 parts of 70# base asphalt and 20 parts of the green high-viscosity and toughness asphalt modifier prepared in the first part of this embodiment.
[0146] The preparation method comprises the following steps:
[0147] (1) heating the base asphalt in an oven at 140°C for 30 minutes;
[0148] (2) Take out the melted base asphalt and place it on an electromagnetic heating device, add the green high-viscosity and toughness asphalt modifier into the base asphalt, stir it manually for 15 minutes, and control the temperature at 175°C;
[0149] (3) After preliminary manual stirring, the modified asphalt was subjected to high-speed shearing at a rate of 6000 r / min for 20 minutes with the temperature controlled at 175°C;
[0150] (4) using a high-speed agitator to further disperse the modified asphalt after high-speed shearing, with the dispersion time controlled at 10 minutes, the rotation speed controlled at 500 r / min, and the temperature controlled at 185° C.;
[0151] (5) The prepared modified asphalt is placed in a closed oven for development for 60 minutes at a temperature of 185° C. to obtain the green high-viscosity and tough modified asphalt.
[0152] 3. This embodiment also provides a method for preparing green high-viscosity and high-toughness asphalt concrete. The asphalt concrete comprises the following raw material components by weight: 6 parts of the green high-viscosity and high-toughness modified asphalt prepared in the second part of this embodiment, 94 parts of aggregate, and 6 parts of mineral powder; the aggregate and mineral powder are configured according to the AC-13 dense-graded asphalt mixture mineral grading shown in Table 1, the void ratio is controlled at 3-6%, and the sieve size of the mineral powder is less than 0.075 mm.
[0153] The specific preparation method is shown in Example 1.
[0154] Comparative Example 1
[0155] The difference from Example 1 is that this comparative example 1 adopts a one-time melt extrusion method. The specific preparation method is as follows:
[0156] 1. Preparation of asphalt modifier
[0157] The modifier includes the following raw material components in parts by weight: 232 parts of a waste rubber and plastic mixture, specifically 129 parts of waste rubber powder with a particle size of 60 mesh (rubber hydrocarbon content>50%), 103 parts of waste polyethylene with a particle size of 10 mesh; 4 parts of nano-organic montmorillonite; 28 parts of aromatic oil (aromatic content greater than 80%).
[0158] The preparation method is a one-time melt blending and extrusion preparation, comprising the following steps:
[0159] First, the waste rubber and plastic mixture, nano-organic montmorillonite and aromatic oil in the above weight parts are weighed and mixed evenly in a high-speed mixer. The speed of the high-speed mixer is controlled at 450 r / min and the mixing time is controlled at 15 minutes.
[0160] Then, it is extruded through a twin-screw extruder, cooled in a water tank, and then pulled to a granulator for primary granulation to obtain an asphalt modifier. The extruder barrel includes a feed section, a discharge section, and 7 intermediate sections. The temperatures of each section from the feed end to the discharge end are 170°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 175°C, 170°C, respectively. The screw speed is 120r / min, and the pelletizer speed is 200 / min; the particle size of the asphalt modifier is controlled to be 10-15 meshes.
[0161] 2. Preparation of modified asphalt
[0162] According to the method of Example 1, modified asphalt was prepared by using 85 parts of 70# base asphalt and 15 parts of the asphalt modifier prepared in the second part of this example.
[0163] 3. This embodiment also provides a method for preparing asphalt concrete. Wherein: the asphalt concrete comprises the following raw material components by weight: 5 parts of the modified asphalt prepared in the second embodiment, 94 parts of aggregate, and 6 parts of mineral powder; the aggregate and mineral powder are configured according to the AC-13 dense graded asphalt mixture mineral grading shown in Table 1, the void ratio is controlled at 3-6%, and the sieve size of the mineral powder is less than 0.075 mm. The specific preparation method refers to Example 1.
[0164] Comparative Example 2:
[0165] The modifier adopts the representative Japanese high-viscosity modifier TPS (TAFPACK-Super) abroad, whose main components are thermoplastic rubber, plasticizer, etc., and is expensive. According to the method of Example 1, by weight, 85 parts of 70# base asphalt and 15 parts of high-viscosity asphalt modifier TPS are used to prepare modified asphalt.
[0166] This embodiment also provides a method for preparing asphalt concrete. Wherein: the asphalt concrete comprises the following raw material components by weight: 5 parts of the modified asphalt prepared in this embodiment, 94 parts of aggregate, and 6 parts of mineral powder; the aggregate and the mineral powder are configured according to the gradation of the AC-13 dense-graded asphalt mixture mineral material shown in Table 1, the void ratio is controlled at 3-6%, and the sieve size of the mineral powder is less than 0.075 mm. The specific preparation method refers to Example 1.
[0167] Performance Test:
[0168] 1. The microstructure of the green high-viscosity and toughness modified asphalt prepared in Examples 1 to 4 and the microstructure of the modified asphalt prepared in Comparative Examples 1 and 2 were characterized using a fluorescence microscope.
[0169] Figure 1 to Figure 4 The microstructure diagrams of the modified asphalt prepared in Examples 1 to 4 are respectively. Figure 5 The microstructure of the modified asphalt of Comparative Example 1 is shown in FIG. Figure 6 This is the microstructure diagram of the modified asphalt of Comparative Example 2. Figure 1 to Figure 6 The medium black is the base asphalt and the white is the asphalt modifier.
[0170] from Figure 1 to Figure 4 It can be seen that the four green high-viscosity and high-toughness asphalt modifiers prepared in the embodiments of the present invention are evenly dispersed in the matrix asphalt and form a stable three-dimensional spatial network structure, thereby greatly improving the comprehensive performance of the asphalt.
[0171] From the comparative Figure 5 , 6 It can be seen that the asphalt modifiers prepared in Comparative Examples 1 and 2 are not evenly dispersed in the base asphalt, and the modifier particles are agglomerated, which will affect the performance of the modified asphalt.
[0172] 2. The present invention tests the melt mass flow rate of the asphalt modifiers of Examples 1 to 4 and Comparative Examples 1 and 2 according to "Determination of Melt Mass Flow Rate (MFR) and Melt Volume Flow Rate (MVR) of Plastic Thermoplastics Part 1: Standard Method" (GB / T3682.1-2018). The key indicators of the modified asphalt prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were tested using the relevant test methods in the "Test Specifications for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011).
[0173] 3. The asphalt concrete prepared in the above-mentioned Examples 1 to 4 and Comparative Examples 1 and 2 is placed in a rutting forming instrument for forming, and a rutting plate with a size of 300 mm in length, 300 mm in width, and 50 mm in height is obtained for standby use, and is used to test and evaluate the low temperature performance of the asphalt concrete. The formed rutting plate is further cut into a prismatic beam with a length of 250 mm ± 2.0 mm, a width of 30 mm ± 2.0 mm, and a height of 35 mm ± 2.0 mm, and is used for standby use, and is used to test and evaluate the high temperature performance of the asphalt concrete. The high and low temperature performance indicators of the asphalt concrete are tested by the relevant test methods in the "Testing Rules for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011).
[0174] The test results are shown in Table 1.
[0175] Table 1 Test results of performance indicators of asphalt modifiers, modified asphalt and asphalt concrete prepared in Examples 1-4 and Comparative Examples 1-2
[0176]
[0177]
[0178] Note: Technical requirements refer to the technical requirements of "Technical Specifications for Preventive Maintenance of Highway Asphalt Pavement" (JTG / T 5142-01-2021) and "Technical Specifications for Construction of Highway Asphalt Pavement" (JTG / T 5142-01-2021)
[0179] From the test results in Table 1, it can be seen that the green high-viscosity and tough asphalt modifier provided by the present invention has excellent flow properties and processing properties, laying the foundation for the preparation of modified asphalt in the later stage. The developed green high-viscosity and tough asphalt has excellent construction and workability, because it forms a stable three-dimensional spatial network structure, and has excellent storage stability, high and low temperature rheological properties, anti-aging properties and bonding properties. The asphalt concrete further prepared has excellent high and low temperature road performance, and can thus significantly improve the service life of traditional asphalt pavement.
[0180] The above descriptions are only some preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A green high-viscosity and high-toughness asphalt modifier, characterized in that: The raw material components include the following parts by weight: 70~232 parts of waste rubber and plastic mixture; 4-10 parts of nano clay material; Compatibilizer 15~50 parts; The waste rubber and plastic mixture is composed of waste rubber and waste plastic, the mass ratio of waste rubber to waste plastic is 1:0.8-1.5; the waste rubber is waste rubber powder, the particle size of which is 40-120 meshes, and the rubber hydrocarbon content is greater than 50%; the waste plastic is waste polyethylene particles or waste polypropylene particles, the particle size of which is 10-15 meshes; The nano-clay material includes at least one of nano-organic montmorillonite, nano-rectorite, and nano-vermiculite; The method is prepared by a secondary melt blending extrusion method, which specifically comprises the following steps: (1) Preparation of masterbatch by melt blending and extrusion: nano-clay material, waste rubber and plastic mixture, and compatibilizer are weighed in a mass ratio of 1:2-4:1-2, mixed at high speed, and extruded and granulated to obtain the masterbatch; (2) Preparation of asphalt modifier by secondary melt blending and extrusion: the waste rubber and plastic mixture, the masterbatch obtained in step (1), and the compatibilizer are uniformly mixed at a mass ratio of 5-9:1-5:1-3 at high speed, and then extruded and granulated for a secondary time to obtain the asphalt modifier.
2. The green high-viscosity and tough asphalt modifier according to claim 1, characterized in that: The compatibilizer is aromatic oil, and the aromatic content thereof is greater than 80%.
3. The green high-viscosity and tough asphalt modifier according to claim 1, characterized in that: The high-speed mixing in step (1) is carried out in a high-speed mixer, the rotation speed of the high-speed mixer is controlled at 300-450 r / min, and the time is controlled at 15-20 minutes.
4. The green high-viscosity and tough asphalt modifier according to claim 1, characterized in that: The high-speed mixing in step (2) is carried out in a high-speed mixer, the rotation speed of the high-speed mixer is controlled at 300-450 r / min, and the time is controlled at 15-20 minutes.
5. The green high-viscosity and high-toughness asphalt modifier according to claim 1, characterized in that: The extrusion process of step (1) is carried out by a twin-screw extruder. The barrel of the twin-screw extruder of step (1) includes a feed section, a discharge section and at least one intermediate section. The temperature of the feed section and the discharge section is controlled at 170° C., the temperature of the intermediate section is controlled at 175° C., and the screw speed is 100-180 r / min.
6. The green high-viscosity and high-toughness asphalt modifier according to claim 1, characterized in that: The extrusion process of step (2) is carried out by a twin-screw extruder. The barrel of the twin-screw extruder of step (2) includes a feed section, a discharge section and at least one intermediate section. The temperature of the feed section and the discharge section is controlled at 170° C., the temperature of the intermediate section is controlled at 175° C., and the screw speed is 100-180 r / min.
7. The green high-viscosity and high-toughness asphalt modifier according to claim 1, characterized in that: Step (1) the extruded material is cooled in a water tank and then pulled to a granulator for primary granulation, with the rotation speed of the granulator being 200-400 r / min; The extruded material in step (2) is cooled in a water tank and then pulled to a granulator for secondary granulation. The rotation speed of the granulator is also 200-400 r / min.
8. The green high-viscosity and tough asphalt modifier according to claim 1, characterized in that: The particle size of the masterbatch obtained in step (1) is controlled within the range of 10-15 meshes; the particle size of the asphalt modifier obtained in step (2) is controlled within the range of 10-15 meshes.
9. A green, highly viscous and tough modified asphalt, characterized in that: It comprises base asphalt and the green high-viscosity and toughness asphalt modifier described in any one of claims 1-8, and the mass ratio of the green high-viscosity and toughness asphalt modifier to the base asphalt is 15-20:80-85.
10. The method for preparing green high-viscosity and high-toughness modified asphalt according to claim 9, characterized in that: The specific steps include: (1) The base asphalt is heated until it melts; (2) taking out the melted base asphalt, adding the green high-viscosity and toughness asphalt modifier into the base asphalt according to a preset ratio, controlling the temperature at 175-180° C., and initially stirring; (3) After initial stirring, the mixed material is subjected to high-speed shearing for 20 to 30 minutes, and the temperature is controlled at 175 to 180°C; (4) Afterwards, high-speed stirring and dispersion is performed at a speed of 300-500 r / min, the dispersion time is controlled within 10-15 minutes, and the temperature is controlled within 175-180°C; (5) Finally, the material obtained in step (4) is kept warm at 175-185°C and sealed for development for 60-70 minutes to obtain the modified asphalt.
11. The preparation method according to claim 10, characterized in that: In step (1), the base asphalt is heated at 135° C. to 140° C. for 30 to 40 minutes until it melts; The high-speed shear rate in step (2) is 4500-6000 r / min.
12. An asphalt concrete, characterized in that: It comprises the green high-viscosity and toughness modified asphalt described in claim 9 or the green high-viscosity and toughness modified asphalt obtained by any of the methods described in claims 10-11, and mineral material; the green high-viscosity and toughness modified asphalt accounts for 5% to 6% of the weight of the mineral material.
13. The asphalt concrete according to claim 12, characterized in that: The mineral material includes aggregate and mineral powder, and the void ratio of the mineral material is controlled at 3-6%.