A process for separating nickel and cobalt from cobalt raffinate

Through the coordination of sodium chloride and hydrochloric acid, combined with the hydrogen bonding of P204 and quaternary ammonium salt, the problem of incomplete separation of cobalt and nickel is solved, efficient extraction and recycling of cobalt is achieved, and environmental pollution is reduced.

CN118241047BActive Publication Date: 2024-11-29YANGJIANG FEDERAL METAL CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410367882.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-29
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

During the wet smelting process of cobalt nickel, the wastewater generated contains precious metals such as Co and Ni. The existing separation method requires long-term ventilation and a large number of oxidants. It is difficult to completely oxidize the divalent cobalt, resulting in incomplete separation and resource loss and environmental pollution.

Method used

Through the coordination between chloride ions in sodium chloride and hydrochloric acid and metal ions, combined with hydrogen bonding between P204 and quaternary ammonium salt, the extraction efficiency of cobalt is improved. The preparation methods of extract liquid include ultrasonic treatment, temperature control reaction and acidity The solution is stripped step, and cobalt and nickel are separated.

Benefits of technology

It significantly improves the extraction rate and separation efficiency of cobalt, reduces environmental pollution, and achieves efficient cobalt recovery.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a process for separating nickel and cobalt from cobalt raffinate, and belongs to the technical field of cobalt recovery. The process comprises the following steps: S1, adding sodium chloride to the cobalt raffinate and stirring evenly, adding an extracting liquid and mixing, adjusting the pH value and performing extraction, and obtaining a loaded organic phase and a decontamination liquid after separation; S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt liquid; the present invention improves the extraction efficiency of cobalt by combining the coordination of chloride ions in sodium chloride and hydrochloric acid with metal ions and the mutual hydrogen bonding and synergistic enhancement between P204, quaternary ammonium salt and N235.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cobalt recovery and relates to a process for separating nickel and cobalt from cobalt raffinate. Background Art

[0002] In the hydrometallurgical process of cobalt and nickel, a large amount of waste water and waste slag are often produced, which contain Co, Ni and a small amount of Fe, Cu, Pb, Cr, Mn, etc. The discharge of such waste water not only causes the loss of precious metal resources, but also causes serious pollution to the environment.

[0003] Therefore, it is of great significance to treat and comprehensively utilize cobalt-nickel-containing wastewater. Commonly used cobalt-nickel separation methods include chemical precipitation, ion exchange, colloidal flotation and solvent extraction. Solvent extraction is used to separate cobalt and nickel. Generally, divalent cobalt is first oxidized into trivalent cobalt, and then forms a stable coordinated cation with some suitable ligands (such as ammonium ions) so that cobalt is not extracted and separated from nickel. The disadvantage of this method is that it requires long-term ventilation and the addition of a large amount of oxidant, and it is not easy to completely oxidize divalent cobalt. In the wastewater discharged from the smelter, Co 2+ and Ni 2+ In the chloride system, the two ions have the same valence and similar radius, and their affinities for ion exchange resins are slightly different, so direct separation using general methods is not thorough. Summary of the invention

[0004] The object of the present invention is to provide a process for separating nickel and cobalt from cobalt raffinate. The present invention improves the extraction efficiency of cobalt by combining the coordination effect of chloride ions in sodium chloride and hydrochloric acid with metal ions and the mutual hydrogen bonding effect and synergistic enhancement between P204, quaternary ammonium salt and N235.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A process for separating nickel and cobalt from a cobalt raffinate, the process comprising the following steps:

[0007] S1. After adding sodium chloride to the cobalt raffinate and stirring evenly, adding the extracting liquid and mixing, adjusting the pH value and performing extraction, and after separation, obtaining a loaded organic phase and a de-impurity liquid; in this step, the purpose is to separate cobalt and nickel, the organic phase mainly contains cobalt ions, the de-impurity liquid mainly contains nickel ions, and the de-impurity liquid can be used for nickel extraction and recovery;

[0008] S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt solution;

[0009] The method for preparing the extract comprises the following steps:

[0010] 1) After ultrasonic treatment of P204, quaternary ammonium salt is added, stirred and mixed, temperature controlled reaction is performed, sulfonated kerosene is added, mixed, sodium bicarbonate solution is added, stirred evenly, allowed to stand, the lower organic phase is separated and washed to obtain an ionic liquid;

[0011] 2) After adding sulfonated kerosene and 2-octanol to N235 and mixing, hydrochloric acid solution is added and ultrasonically mixed, after standing to separate the water phase, ionic liquid is added and stirred to obtain an extract.

[0012] As a preferred technical solution of the present invention, in step S1, the condition for adjusting the pH value is to adjust the pH value to 5.0-5.3; the conditions for the extraction are: an O / A ratio of 1, a rotation speed of 180-200 r / min, a temperature of 25°C, and extraction for 20-25.5 min; the dosage ratio of the cobalt raffinate and sodium chloride is 1L:9.0-10.5mol.

[0013] As a preferred technical solution of the present invention, in step S2, the acidic solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 4 mol / L; the stripping conditions are at an O / A ratio of 1, a temperature of 25°C, and stripping for 20 minutes.

[0014] As a preferred technical solution of the present invention, in step 1), the ultrasonic treatment is carried out at a frequency of 90-120 kHz for 15-21 min.

[0015] As a preferred technical solution of the present invention, in step 1), the temperature control reaction conditions are 17-23°C, 180-210 r / min, and a reaction time of 10-16 min.

[0016] As a preferred technical solution of the present invention, in step 1), the stirring time is 15-18 minutes; the standing time is 30-45 minutes; and the washing condition is washing 3 times with deionized water.

[0017] As a preferred technical solution of the present invention, in step 1), the usage ratio of the quaternary ammonium salt, P204, sulfonated kerosene and sodium bicarbonate solution is 10.0-11.5 g: 8.3-8.6 mL: 25 mL: 50-56 mL.

[0018] As a preferred technical solution of the present invention, in step 1), the concentration of the sodium bicarbonate solution is 0.5 mol / L; and the quaternary ammonium salt is methyl trioctyl ammonium chloride.

[0019] As a preferred technical solution of the present invention, in step 2), the concentration of the hydrochloric acid solution is 3 mol / L; the ultrasonic mixing condition is at a frequency of 300-400 kHz and ultrasonic treatment for 5-8 min.

[0020] As a preferred technical solution of the present invention, in step 2), the mass ratio of N235, sulfonated kerosene, 2-octanol, hydrochloric acid solution and ionic liquid is 1.0-1.3:5:0.50-0.62:3.0-3.3:2.4-3.0.

[0021] As a preferred technical solution of the present invention,.

[0022] Beneficial effects of the present invention:

[0023] (1) The present invention can improve the extraction rate of the target cobalt ions by the extracting solution through the coordination effect between the chloride ions in sodium chloride and hydrochloric acid and the metal ions; at the same time, as a leaching agent, hydrochloric acid can also reduce high-valent metal ions to low-valent metal ions, which is beneficial to the separation and recovery of cobalt.

[0024] (2) The ionic liquid is synthesized by combining the hydrophobic anion in P204 with the quaternary ammonium cation in the quaternary ammonium salt and used to extract the metal cobalt ion. Since both the anion and the cation can participate in the extraction process, the strong internal synergistic effect can significantly improve the distribution ratio of the target metal ion.

[0025] (3) The synergistic extraction mechanism of N235 and P204 is that the hydrogen bond formed between the two will lead to the breakage of the P204 dimer, thereby improving the extraction efficiency of cobalt.

[0026] (4) N235 can exchange H with P204 when extracting metal ions + The reaction keeps the pH of the aqueous phase at a low level, thereby ensuring efficient extraction of the target metal cobalt ions. DETAILED DESCRIPTION

[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0028] Example 1

[0029] A process for separating nickel and cobalt from a cobalt raffinate, the process comprising the following steps:

[0030] S1. After adding sodium chloride to the cobalt raffinate and stirring evenly, adding the extracting liquid and mixing, adjusting the pH value and performing extraction, and obtaining a loaded organic phase after separation; wherein the condition for adjusting the pH value is to adjust the pH value to 5.0; the conditions for the extraction are to extract for 20 minutes at a phase O / A ratio of 1, a rotation speed of 180 r / min, a temperature of 25° C.; the amount ratio of the cobalt raffinate and sodium chloride is 1L:9.0mol;

[0031] S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt solution; wherein the acidic solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 4 mol / L; the stripping conditions are at a ratio of O / A of 1, a temperature of 25° C., and stripping for 20 min;

[0032] The method for preparing the extract comprises the following steps:

[0033] 1) After ultrasonic treatment of P204, methyl trioctyl ammonium chloride is added, stirred and mixed, temperature controlled reaction is carried out, sulfonated kerosene is added and mixed, sodium bicarbonate solution is added, stirred evenly, allowed to stand, the lower organic phase is separated and taken out, and the ionic liquid is obtained after washing; wherein, the ultrasonic treatment condition is at a frequency of 90kHz and an ultrasonic treatment time of 15min; the temperature control reaction condition is at a temperature of 17°C and a speed of 180r / min and a reaction time of 10min; the stirring time is 15min; the standing time is 30min; the washing condition is washing with deionized water for 3 times; the dosage ratio of the quaternary ammonium salt, P204, sulfonated kerosene and sodium bicarbonate solution is 10.0g:8.3mL:25mL:50mL; the concentration of the sodium bicarbonate solution is 0.5mol / L;

[0034] 2) After adding sulfonated kerosene and 2-octanol to N235 and mixing, hydrochloric acid solution is added and ultrasonically mixed, after standing to separate the dehydrated phase, ionic liquid is added and stirred to obtain an extract; wherein the concentration of the hydrochloric acid solution is 3 mol / L; the ultrasonic mixing condition is at a frequency of 300 kHz and ultrasonic treatment for 5 min; the mass ratio of N235, sulfonated kerosene, 2-octanol, hydrochloric acid solution and ionic liquid is 1.0:5:0.50:3.0:2.4.

[0035] Example 2

[0036] A process for separating nickel and cobalt from a cobalt raffinate, the process comprising the following steps:

[0037] S1. After adding sodium chloride to the cobalt raffinate and stirring evenly, adding the extracting liquid and mixing, adjusting the pH value and performing extraction, and obtaining a loaded organic phase after separation; wherein the condition for adjusting the pH value is to adjust the pH value to 5.1; the conditions for the extraction are to extract for 22 minutes at a relative O / A ratio of 1, a rotation speed of 187 r / min, a temperature of 25° C.; and the amount ratio of the cobalt raffinate and sodium chloride is 1L:9.5mol;

[0038] S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt solution; wherein the acidic solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 4 mol / L; the stripping conditions are at a ratio of O / A of 1, a temperature of 25° C., and stripping for 20 min;

[0039] The method for preparing the extract comprises the following steps:

[0040] 1) After ultrasonic treatment of P204, methyl trioctyl ammonium chloride is added, stirred and mixed, temperature controlled reaction is performed, sulfonated kerosene is added and mixed, sodium bicarbonate solution is added and stirred evenly, standing, separating and removing the lower organic phase, and washing to obtain an ionic liquid; wherein, the ultrasonic treatment condition is at a frequency of 100kHz and an ultrasonic treatment time of 17 minutes; the temperature control reaction condition is at a temperature of 19°C and a speed of 190r / min and a reaction time of 12 minutes; the stirring time is 16 minutes; the standing time is 35 minutes; the washing condition is washing 3 times with deionized water; the dosage ratio of the quaternary ammonium salt, P204, sulfonated kerosene and sodium bicarbonate solution is 10.5g:8.4mL:25mL:52mL; the concentration of the sodium bicarbonate solution is 0.5mol / L;

[0041] 2) After adding sulfonated kerosene and octanol to N235 and mixing, hydrochloric acid solution is added and ultrasonically mixed, after standing to separate the dehydrated phase, ionic liquid is added and stirred to obtain an extract; wherein the concentration of the hydrochloric acid solution is 3 mol / L; the ultrasonic mixing condition is at a frequency of 333 kHz and ultrasonic treatment for 6 min; the mass ratio of N235, sulfonated kerosene, octanol, hydrochloric acid solution and ionic liquid is 1.1:5:0.54:3.1:2.6.

[0042] Example 3

[0043] A process for separating nickel and cobalt from a cobalt raffinate, the process comprising the following steps:

[0044] S1. After adding sodium chloride to the cobalt raffinate and stirring evenly, adding the extracting liquid and mixing, adjusting the pH value and performing extraction, and obtaining a loaded organic phase after separation; wherein the condition for adjusting the pH value is to adjust the pH value to 5.2; the conditions for the extraction are to extract for 24 minutes at a phase O / A ratio of 1, a rotation speed of 193 r / min, a temperature of 25° C.; and the amount ratio of the cobalt raffinate to the sodium chloride is 1 L:10 mol;

[0045] S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt solution; wherein the acidic solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 4 mol / L; the stripping conditions are at a ratio of O / A of 1, a temperature of 25° C., and stripping for 20 min;

[0046] The method for preparing the extract comprises the following steps:

[0047] 1) After ultrasonic treatment of P204, methyl trioctyl ammonium chloride is added and stirred and mixed, and the temperature is controlled to react. After adding sulfonated kerosene and mixing, sodium bicarbonate solution is added and stirred evenly, and the mixture is allowed to stand. The lower organic phase is separated and washed to obtain an ionic liquid; wherein the ultrasonic treatment condition is 19 minutes at a frequency of 110kHz; the temperature control reaction condition is 14 minutes at a temperature of 21°C and a speed of 200r / min; the stirring time is 17 minutes; the standing time is 40 minutes; the washing condition is 3 times of washing with deionized water; the dosage ratio of the quaternary ammonium salt, P204, sulfonated kerosene and sodium bicarbonate solution is 11g:8.5mL:25mL:54mL; the concentration of the sodium bicarbonate solution is 0.5mol / L;

[0048] 2) After adding sulfonated kerosene and octanol to N235 and mixing, hydrochloric acid solution is added and ultrasonically mixed, after standing to separate the dehydrated phase, ionic liquid is added and stirred to obtain an extract; wherein the concentration of the hydrochloric acid solution is 3 mol / L; the ultrasonic mixing condition is at a frequency of 367 kHz and ultrasonic treatment for 7 min; the mass ratio of N235, sulfonated kerosene, octanol, hydrochloric acid solution and ionic liquid is 1.2:5:0.58:3.2:2.8.

[0049] Example 4

[0050] A process for separating nickel and cobalt from a cobalt raffinate, the process comprising the following steps:

[0051] S1. After adding sodium chloride to the cobalt raffinate and stirring evenly, adding the extracting liquid and mixing, adjusting the pH value and performing extraction, and obtaining a loaded organic phase after separation; wherein the condition for adjusting the pH value is to adjust the pH value to 5.3; the conditions for the extraction are to extract for 25.5 min at a ratio of O / A of 1, a rotation speed of 200 r / min, a temperature of 25°C; and the amount ratio of the cobalt raffinate and sodium chloride is 1 L:10.5 mol;

[0052] S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt solution; wherein the acidic solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 4 mol / L; the stripping conditions are at a ratio of O / A of 1, a temperature of 25° C., and stripping for 20 min;

[0053] The method for preparing the extract comprises the following steps:

[0054] 1) After ultrasonic treatment of P204, methyl trioctyl ammonium chloride is added, stirred and mixed, temperature controlled reaction is performed, sulfonated kerosene is added and mixed, sodium bicarbonate solution is added, stirred evenly, allowed to stand, the lower organic phase is separated and taken out, and the ionic liquid is obtained after washing; wherein, the ultrasonic treatment condition is at a frequency of 120kHz and an ultrasonic treatment time of 21min; the temperature control reaction condition is at a temperature of 23°C and a speed of 210r / min and a reaction time of 16min; the stirring time is 18min; the standing time is 45min; the washing condition is washing 3 times with deionized water; the dosage ratio of the quaternary ammonium salt, P204, sulfonated kerosene and sodium bicarbonate solution is 11.5g:8.6mL:25mL:56mL; the concentration of the sodium bicarbonate solution is 0.5mol / L;

[0055] 2) After adding sulfonated kerosene and 2-octanol to N235 and mixing, hydrochloric acid solution is added and ultrasonically mixed, after standing to separate the dehydrated phase, ionic liquid is added and stirred to obtain an extract; wherein the concentration of the hydrochloric acid solution is 3 mol / L; the ultrasonic mixing condition is at a frequency of 400 kHz and ultrasonic treatment for 8 min; the mass ratio of N235, sulfonated kerosene, 2-octanol, hydrochloric acid solution and ionic liquid is 1.3:5:0.62:3.3:3.0.

[0056] Comparative Example 1

[0057] Compared with Example 2, the difference is that sodium chloride is not added, and the other components, preparation steps and parameters are the same.

[0058] Comparative Example 2

[0059] Compared with Example 2, the difference is that P204 is not used in Comparative Example 2, and the other components, preparation steps and parameters are the same.

[0060] Comparative Example 3

[0061] Compared with Example 2, the difference is that Comparative Example 3 does not use methyl trioctyl ammonium chloride, and the other components, preparation steps and parameters are the same.

[0062] Comparative Example 4

[0063] Compared with Example 2, the difference is that Comparative Example 4 does not use N235, and the other components, preparation steps and parameters are the same.

[0064] Comparative Example 5

[0065] Compared with Example 2, the difference is that comparative example 5 does not use 2-octanol, and the other components, preparation steps and parameters are the same.

[0066] The cobalt yields of Examples 1-4 and Comparative Examples 1-5 were tested respectively, and the test results are shown in Table 1.

[0067] Table 1

[0068] Cobalt yield (%) Example 1 88.6 Example 2 89.8 Example 3 88.4 Example 4 89.2 Comparative Example 1 67.5 Comparative Example 2 71.2 Comparative Example 3 76.4 Comparative Example 4 74.8 Comparative Example 5 82.5

[0069] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-5, the yield of cobalt in Examples 1-4 of the present invention is significantly better than that in Comparative Examples 1-5.

[0070] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A process for separating nickel and cobalt from cobalt raffinate, characterized in that: The process comprises the following steps: S1. After adding sodium chloride to the cobalt raffinate and stirring evenly, adding the extract and mixing, adjusting the pH value and performing extraction, and after separation, obtaining a loaded organic phase and a decontamination liquid; S2, adding an acidic solution to the loaded organic phase for stripping to obtain a cobalt solution; The method for preparing the extract comprises the following steps: 1) P204 is ultrasonically treated, and then a quaternary ammonium salt is added, stirred and mixed, and the temperature is controlled to react. After adding sulfonated kerosene and mixing, a sodium bicarbonate solution is added and stirred evenly, and the mixture is allowed to stand, and the lower organic phase is separated and washed to obtain an ionic liquid; the temperature control reaction conditions are 17-23°C, 180-210r / min, and the reaction time is 10-16min; the amount ratio of the quaternary ammonium salt, P204, sulfonated kerosene and sodium bicarbonate solution is 10.0-11.5g:8.3-8.6mL:25mL:50-56mL; the quaternary ammonium salt is methyl trioctyl ammonium chloride; 2) After adding sulfonated kerosene and 2-octanol to N235 and mixing, hydrochloric acid solution is added and ultrasonically mixed. After standing to separate the water phase, ionic liquid is added and stirred to obtain an extract.

2. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step S1, the condition for adjusting the pH value is to adjust the pH value to 5.0-5.3; the conditions for the extraction are: an O / A ratio of 1, a rotation speed of 180-200 r / min, a temperature of 25°C, and extraction for 20-25.5 min; the usage ratio of the cobalt raffinate and sodium chloride is 1L:9.0-10.5 mol.

3. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step S2, the acidic solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 4 mol / L; the stripping conditions are: a ratio of O / A of 1, a temperature of 25°C, and stripping for 20 minutes.

4. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step 1), the ultrasonic treatment is carried out at a frequency of 90-120 kHz for 15-21 min.

5. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step 1), the stirring time is 15-18 minutes; the standing time is 30-45 minutes; and the washing condition is washing 3 times with deionized water.

6. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step 1), the concentration of the sodium bicarbonate solution is 0.5 mol / L.

7. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step 2), the concentration of the hydrochloric acid solution is 3 mol / L; the ultrasonic mixing condition is at a frequency of 300-400 kHz and ultrasonic treatment for 5-8 min.

8. A process for separating nickel and cobalt from cobalt raffinate according to claim 1, characterized in that: In step 2), the mass ratio of N235, sulfonated kerosene, 2-octanol, hydrochloric acid solution and ionic liquid is 1.0-1.3:5:0.50-0.62:3.0-3.3:2.4-3.0.