Preparation method of biomass-based OLED electronic component packaging adhesive
Through the preparation method of biomass-based OLED electronic components packaging glue, the combination of polyvinyl alcohol modified lignin and other components is used to solve the problem of easy corrosion of OLED devices and insufficient packaging glue performance, and the colorless packaging glue is realized Self-healing function and high viscosity extend service life and improve optical stability.
Patent Information
- Application Number
- CN202410440127.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-04-12
AI Technical Summary
OLED electronic components are prone to corrosion in the presence of air and water, resulting in a reduced service life. The packaging glue needs to have colorless, low molar absorbance, high bonding strength and excellent water and oxygen insulation properties.
The preparation method of biomass-based OLED electronic component packaging glue is adopted, and the colorless preparation is prepared by physical treatment and chemical modification of polyvinyl alcohol modified lignin, combined with epoxy silane, boric acid, avobenzone and nanotitanium dioxide. and improve its viscosity and optical stability through ultraviolet curing technology.
The colorless packaging glue is realized, giving it self-healing function and long service life, improving the viscosity and optical stability of the packaging glue, and avoiding aging and corrosion problems.
Smart Images

Figure CN118256190B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer encapsulation adhesives for OLED devices, and relates to a method for preparing a biomass-based OLED electronic component encapsulation adhesive. Background Art
[0002] In recent years, the application of OLED (organic light-emitting diode) in the fields of new display and solid-state lighting has developed rapidly. Since OLED electronic components are easily corroded in the presence of air and water, the service life of the device is seriously reduced. In order to improve the service life of OLED electronic components, device packaging is an indispensable step. Since the optical performance of OLED electronic components is one of its most important properties, the device must not only have good water and oxygen isolation properties during the packaging process, but also have a low molar absorption coefficient and high bonding strength. Since OLED devices are light-emitting devices, the functional layer, substrate, protective layer, film, packaging glue, etc. of OLED are required to be colorless. In this way, the luminous performance of OLED devices can be guaranteed not to be affected. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a biomass-based OLED electronic component encapsulation adhesive. The encapsulation adhesive prepared by the method is colorless and has high bonding strength.
[0004] The technical solution adopted by the present invention is a method for preparing a biomass-based OLED electronic component encapsulation adhesive, which specifically comprises the following steps:
[0005] Step 1, preparing polyvinyl alcohol modified lignin;
[0006] Step 2, preparing encapsulation glue according to the polyvinyl alcohol-modified lignin prepared in step 1;
[0007] Step 3, UV curing the packaging glue prepared in step 2.
[0008] The present invention is also characterized in that:
[0009] The specific process of step 1 is:
[0010] Step 1.1, taking 10g-50g of broadleaf lignin and dispersing it in 400-2000mL of ethanol / tetrahydrofuran solution and extracting it for 12h-24h to obtain extracted lignin;
[0011] Step 1.2, taking 2g-5g of the extracted lignin and 0.2g-0.5g of sodium sulfonate and dispersing them in 50mL-100mL of deionized water solution, heating and reflux reaction at 60°C-100°C for 12h-36h, cooling to room temperature after the reaction, adding HCl solution with a pH of 2-4 for acidification treatment, and obtaining sulfonated lignin;
[0012] Step 1.3, take 0.5g-1g of sulfonated lignin and 0.2g-0.5g of polyvinyl alcohol, add 0.01-0.02mL of concentrated sulfuric acid and continue stirring for 12-24h to obtain colorless polyvinyl alcohol modified lignin.
[0013] In step 1.3, the molecular weight of the polyvinyl alcohol is 1000-10000.
[0014] The specific process of step 2 is:
[0015] Step 2.1, take 0.5g-1g of polyvinyl alcohol-modified lignin, 0.1g-0.2g of boric acid, and 1-3mL of methyl acrylate, stir and age at room temperature for 3h-6h;
[0016] Step 2.2, adding 0.1g-0.5g of N,N,N',N'-tetracyclyl-4,4'-diaminodiphenylmethane, 0.1g-0.5g of N,N,N',N'-tetracyclyl-4,4'-diaminodimethylsiloxane, and 1-2g of acrylate oligomer to the solution aged in step 2.1, and continuing to stir for 30-60min; Step 2.3, adding 0.1g-0.2g of nano titanium dioxide, 0.01g-0.02g of avobenzone, and 0.01g-0.02g of triphenylsulfonium tetrafluoroborate to the solution obtained in step 2.2, and stirring at room temperature for 30min-60min to obtain a packaging glue.
[0017] The specific process of step 3 is:
[0018] The encapsulation glue prepared in step 2 was dropped onto the polytetrafluoroethylene substrate and evenly coated by spin coating. The operation was repeated 5 times and finally placed in 800mJ / cm 2 -1000 mJ / cm 2 Place it in a UV oven, and after polymerization, peel off the light-cured packaging glue to obtain the product.
[0019] The beneficial effects of the present invention are as follows:
[0020] 1. The present invention uses lignin as raw material, performs physical treatment and chemical modification, obtains colorless and transparent modified lignin, and further prepares OLED device encapsulation glue with epoxy silane, etc. In particular, the self-repairing function of the encapsulation glue gives the encapsulation glue a long service life.
[0021] 2. The present invention uses green, environmentally friendly and renewable lignin as raw material to prepare colorless encapsulation glue. Secondly, a boric acid system is introduced into the encapsulation glue to improve the viscosity of the encapsulation glue on the one hand and give it excellent self-repair and anti-aging properties on the other hand. Finally, avobenzone and nano-titanium dioxide are introduced into the system to improve the optical stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the absorption spectrum of Example 1 of the preparation method of the biomass-based OLED electronic component packaging adhesive of the present invention and Comparative Examples 1-5. DETAILED DESCRIPTION
[0023] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0024] The method for preparing the biomass-based OLED electronic component encapsulation adhesive of the present invention specifically comprises the following steps:
[0025] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0026] Take 10-50g of broadleaf wood lignin, disperse it in 400-2000mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 12-24h to obtain a pale yellow solid powder lignin precursor. Take 2-5g of the extracted lignin precursor and 0.2-0.5g of sodium sulfonate and disperse them in 50-100mL of deionized water solution, and heat and reflux at 60-100℃ for 12-36h. After the reaction is completed, cool it to room temperature, add HCl solution with a pH of 2-4 for acidification, and obtain sulfonated lignin; further take 0.5-1g of sulfonated lignin and 0.2-0.5g of polyvinyl alcohol (molecular weight of 1000-10000), add 0.01-0.02mL of concentrated sulfuric acid and continue stirring for 12-24h to obtain colorless polyvinyl alcohol modified lignin.
[0027] Step 2, preparation of packaging glue, the specific process is as follows:
[0028] First, take 0.5-1g of polyvinyl alcohol-modified lignin, 0.1-0.2g of boric acid, and 1-3mL of methyl acrylate, and stir at room temperature for 3-6h. Secondly, add 0.1-0.5g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.1-0.5g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 1-2g of octanoic acid oligomer to the aged solution, and continue stirring for 30-60min. Finally, continue to add 0.1-0.2g of nano titanium dioxide, 0.01-0.02g of avobenzone, and 0.01-0.02g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 30-60min to obtain encapsulation glue for standby use.
[0029] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0030] Add the encapsulation glue to a 1cmx1cm PTFE substrate, spin coat evenly at 3000r / min, repeat the operation 5 times, and finally put it into 800-1000mJ / cm2 After polymerization, peel off the light-cured encapsulation glue to obtain.
[0031] Example 1
[0032] The method for preparing the biomass-based OLED electronic component encapsulation adhesive of the present invention specifically comprises the following steps:
[0033] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0034] Take 10g of broadleaf wood lignin, disperse it in 400mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 12h to obtain a pale yellow solid powder lignin precursor. Take 2g of the extracted lignin precursor and 0.2g of sodium sulfonate dispersed in 50mL of deionized water solution, and heated to reflux at 60℃ for 12h. After the reaction is completed, cool it to room temperature, add pH 2 HCl solution for acidification, and obtain sulfonated lignin; further take 0.5g of sulfonated lignin and 0.2g of polyvinyl alcohol (molecular weight 1000), add 0.01mL of concentrated sulfuric acid and continue stirring for 12h to obtain colorless polyvinyl alcohol modified lignin.
[0035] Step 2, preparation of packaging glue, the specific process is as follows:
[0036] First, take 0.5g of polyvinyl alcohol-modified lignin, 0.1g of boric acid, and 1mL of methyl acrylate, and stir at room temperature for 3h. Secondly, add 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 1g of octanoic acid oligomer to the aged solution, and continue stirring for 30min. Finally, continue to add 0.1g of nano-titanium dioxide, 0.01g of avobenzone, and 0.01g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 30min to obtain encapsulation glue for standby use.
[0037] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0038] Add the encapsulation glue to a 1cmx1cm PTFE substrate, spin coat it evenly at 3000r / min, repeat the operation 5 times, and finally put it into a UV oven at 800mJ / cm2. After polymerization, peel off the light-cured encapsulation glue to obtain the product.
[0039] Comparative Example 1 (lignin was not extracted with ethanol / tetrahydrofuran, and the prepared encapsulation adhesive was yellow, which did not meet the colorless and transparent requirements)
[0040] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0041] Take 2g of broadleaf lignin and 0.2g of sodium sulfonate dispersed in 50mL of deionized water solution, and heat under reflux at 60℃ for 12h. After the reaction is completed, cool to room temperature, add HCl solution with pH 2 for acidification, and obtain sulfonated lignin; further take 0.5g of sulfonated lignin and 0.2g of polyvinyl alcohol (molecular weight of 1000), add 0.01mL of concentrated sulfuric acid and continue stirring for 12h to obtain yellow polyvinyl alcohol modified lignin.
[0042] Step 2, preparation of packaging glue, the specific process is as follows:
[0043] First, take 0.5g of polyvinyl alcohol-modified lignin, 0.1g of boric acid, and 1mL of methyl acrylate, and stir and age at room temperature for 3h. Secondly, add 0.1g of N,N,N',N'-tetracyclyl-4,4'-diaminodiphenylmethane, 0.1g of N,N,N',N'-tetracyclyl-4,4'-diaminodimethylsiloxane, and 1g of octanoic acid oligomer to the aged solution, and continue stirring for 30min. Finally, continue to add 0.1g of nano-titanium dioxide, 0.01g of avobenzone, and 0.01g of triphenylsulfonium tetrafluoroborate.
[0044] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0045] The encapsulation glue was dripped onto a 1cmx1cm PTFE substrate, and evenly coated at 3000r / min, and the operation was repeated 5 times, and finally placed in a UV oven at 800mJ / cm2. After polymerization, the light-cured encapsulation glue was peeled off and its photophysical properties were tested.
[0046] Comparative Example 2 (boric acid is not added to the encapsulation adhesive, the encapsulation adhesive has low bonding strength and is easily aged, and has poor water and oxygen isolation)
[0047] Step 1, polyvinyl alcohol modified lignin, specifically comprising the following steps:
[0048] Take 10g of broadleaf lignin, disperse it in 400mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 12h to obtain a pale yellow solid powder precursor. Take 2g of the extracted lignin precursor and 0.2g of sodium sulfonate dispersed in 50mL of deionized water solution, and heated to reflux at 60℃ for 12h. After the reaction is completed, cool it to room temperature, add pH 2 HCl solution for acidification, and obtain sulfonated lignin; further take 0.5g of sulfonated lignin and 0.2g of polyvinyl alcohol (molecular weight 1000), add 0.01mL of concentrated sulfuric acid and continue stirring for 12h to obtain colorless polyvinyl alcohol modified lignin.
[0049] Step 2, preparation of packaging glue, the specific process is as follows:
[0050] First, take 0.5g of polyvinyl alcohol-modified lignin and 1mL of methyl acrylate, stir and age at room temperature for 3h. Secondly, add 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 1g of octanoic acid oligomer to the aged solution, and continue to stir for 30min. Finally, continue to add 0.1g of nano-titanium dioxide, 0.01g of avobenzone, and 0.01g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 30min to obtain encapsulation glue for use.
[0051] Step 3, UV curing of the encapsulation adhesive, specifically includes the following steps:
[0052] Add the encapsulation glue to a 1cmx1cm PTFE substrate, spin coat it evenly at 3000r / min, repeat the operation 5 times, and finally put it into a UV oven at 800mJ / cm2. After polymerization, peel off the light-cured encapsulation glue to obtain the product.
[0053] Comparative Example 3 (Nano titanium dioxide is not added to the encapsulation adhesive, and the encapsulation adhesive has low friction resistance and is prone to aging)
[0054] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0055] Take 10g of broadleaf lignin, disperse it in 400mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 12h to obtain a pale yellow solid powder precursor. Take 2g of the extracted lignin precursor and 0.2g of sodium sulfonate and disperse them in 50mL of deionized water solution, heat and reflux at 60℃ for 12h. After the reaction is completed, cool it to room temperature and add HCl solution with a pH of 2 for acidification. Further take 0.5g of sulfonated lignin and 0.2g of polyvinyl alcohol (molecular weight of 1000), add 0.01mL of concentrated sulfuric acid and continue stirring for 12h to obtain colorless polyvinyl alcohol modified lignin.
[0056] Step 2, preparation of packaging glue, the specific process is as follows:
[0057] First, take 0.5g of polyvinyl alcohol-modified lignin, 0.1g of boric acid, and 1mL of methyl acrylate, and stir at room temperature for 3h. Secondly, add 0.1g of N,N,N',N'-tetracyclyl-4,4'-diaminodiphenylmethane, 0.1g of N,N,N',N'-tetracyclyl-4,4'-diaminodimethylsiloxane, and 1g of octanoic acid oligomer to the aged solution, and continue stirring for 30min. Finally, continue to add 0.01g of avobenzone and 0.01g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 30min to obtain encapsulation glue for use.
[0058] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0059] The encapsulation glue was dripped onto a 1cmx1cm PTFE substrate, and evenly coated at 3000r / min, and the operation was repeated 5 times, and finally placed in a UV oven at 800mJ / cm2. After polymerization, the light-cured encapsulation glue was peeled off and its photophysical properties were tested.
[0060] Comparative Example 4 (Avobenzone was not added to the encapsulating adhesive, and the encapsulating adhesive was prone to aging)
[0061] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0062] Take 10g of broadleaf wood lignin, disperse it in 400mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 12h to obtain a light yellow solid powder. Take 2g of the extracted lignin and 0.2g of sodium sulfonate and disperse them in 50mL of deionized water solution, heat and reflux at 60℃ for 12h. After the reaction is completed, cool it to room temperature and add HCl solution with a pH of 2 for acidification. Further take 0.5g of sulfonated lignin and 0.2g of polyvinyl alcohol (molecular weight of 1000), add 0.01mL of concentrated sulfuric acid and continue stirring for 12h to obtain colorless polyvinyl alcohol modified lignin.
[0063] Step 2, preparation of packaging glue, the specific process is as follows:
[0064] First, take 0.5g of polyvinyl alcohol-modified lignin, 0.1g of boric acid, and 1mL of methyl acrylate, and stir at room temperature for 3h. Secondly, add 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 1g of octanoic acid oligomer to the aged solution, and continue stirring for 30min. Finally, continue to add 0.1g of nano-titanium dioxide and 0.01g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 30min to obtain encapsulation glue for use.
[0065] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0066] Add the encapsulation glue to a 1cmx1cm PTFE substrate, spin coat it evenly at 3000r / min, repeat the operation 5 times, and finally put it into a UV oven at 800mJ / cm2. After polymerization, peel off the light-cured encapsulation glue to obtain the product.
[0067] Comparative Example 5 (lignin is not modified by polyvinyl alcohol, the encapsulation adhesive has low viscosity and is easy to age)
[0068] Step 1, non-polyvinyl alcohol modified lignin, the specific process is as follows:
[0069] Take 10g of broadleaf lignin, disperse it in 400mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 12h to obtain a pale yellow solid powder precursor. Take 2g of the extracted lignin precursor and 0.2g of sodium sulfonate and disperse them in 50mL of deionized water solution, heat and reflux at 60℃ for 12h. After the reaction is completed, cool it to room temperature and add HCl solution with pH 2 for acidification.
[0070] Step 2, preparation of packaging glue, the specific process is as follows:
[0071] First, take 0.5g of non-polyvinyl alcohol modified lignin, 0.1g of boric acid, and 1mL of methyl acrylate, and stir and age at room temperature for 3h. Secondly, add 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.1g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 1g of octanoic acid oligomer to the aged solution, and continue stirring for 30min. Finally, continue to add 0.1g of nano titanium dioxide, 0.01g of avobenzone, and 0.01g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 30min to obtain encapsulation glue for use.
[0072] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0073] Add the encapsulation glue to a 1cmx1cm PTFE substrate, spin coat it evenly at 3000r / min, repeat the operation 5 times, and finally put it into a UV oven at 800mJ / cm2. After polymerization, peel off the light-cured encapsulation glue to obtain the product.
[0074] The results and analysis are shown in Table 1 below:
[0075] Table 1
[0076]
[0077] Optical aging is measured by irradiating the steel with 48W ultraviolet light for 240 hours to determine its mechanical properties. If the mechanical property degradation is greater than 50%, it is considered to be susceptible to aging.
[0078] In Comparative Example 1, the lignin was not drawn before use, and the prepared polyvinyl alcohol-modified lignin was yellow. It was also yellow when applied to the encapsulation adhesive. It had obvious light absorption in the wavelength range of 400-500nm, such as Figure 1 In contrast, Example 1 and Comparative Examples 2-5 have no absorption peak visible light and are colorless and transparent.
[0079] In Comparative Example 2, no boric acid was added. The cured film had poor water and oxygen isolation effects due to the lack of the cross-linking effect of boric acid and was prone to aging due to the lack of dynamic reversible repair.
[0080] In comparative example 3, titanium dioxide is not added, so that light radiation cannot be effectively shielded to avoid aging of the film caused by light-generated free radicals. At the same time, the friction resistance of the film is reduced.
[0081] Comparative Example 4 did not add avobenzone, had poor UV light blocking performance, had no absorption peak at 300-400 nm, and the film was prone to aging.
[0082] In comparative example 5, the lignin was not modified with vinyl alcohol and could not form a self-repairing cross-linking structure with boric acid. The adhesive film was prone to aging and the bonding strength was reduced.
[0083] Example 2
[0084] The method for preparing the biomass-based OLED electronic component encapsulation adhesive of the present invention specifically comprises the following steps:
[0085] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0086] Take 50g of broadleaf wood lignin, disperse it in 2000mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 24h to obtain a pale yellow solid powder lignin precursor. Take 5g of the extracted lignin precursor and 0.5g of sodium sulfonate and disperse them in 100mL of deionized water solution, and heat and reflux at 100℃ for 36h. After the reaction is completed, cool it to room temperature, add pH 4 HCl solution for acidification, and obtain sulfonated lignin; further take 1g of sulfonated lignin and 0.5g of polyvinyl alcohol (molecular weight of 10000), add 0.02mL of concentrated sulfuric acid and continue stirring for 24h to obtain colorless polyvinyl alcohol modified lignin.
[0087] Step 2, preparation of packaging glue, the specific process is as follows:
[0088] First, take 1g of polyvinyl alcohol-modified lignin, 0.2g of boric acid, and 3mL of methyl acrylate, and stir and age at room temperature for 6h. Secondly, add 0.5g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.5g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 2g of octanoic acid oligomer to the aged solution, and continue stirring for 60min. Finally, continue to add 0.2g of nano-titanium dioxide, 0.02g of avobenzone, and 0.02g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 60min to obtain encapsulation glue for use.
[0089] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0090] The encapsulation glue was dropped onto a 1cmx1cm PTFE substrate and evenly coated at 3000r / min. The operation was repeated 5 times and finally placed into 800mJ / cm 2 After polymerization, peel off the light-cured encapsulation glue to obtain.
[0091] Example 3
[0092] The method for preparing the biomass-based OLED electronic component encapsulation adhesive of the present invention specifically comprises the following steps:
[0093] Step 1, polyvinyl alcohol modified lignin, the specific process is as follows:
[0094] Take 30g of broadleaf wood lignin, disperse it in 1000mL of ethanol / tetrahydrofuran (v:v=1:1) solution and extract it for 20h to obtain a pale yellow solid powder lignin precursor. Take 3g of the extracted lignin precursor and 0.3g of sodium sulfonate dispersed in 80mL of deionized water solution, and heated to reflux at 80℃ for 24h. After the reaction is completed, cool it to room temperature, add pH 3 HCl solution for acidification, and obtain sulfonated lignin; further take 0.8g of sulfonated lignin and 0.3g of polyvinyl alcohol (molecular weight 8000), add 0.015mL of concentrated sulfuric acid and continue stirring for 18h to obtain colorless polyvinyl alcohol modified lignin.
[0095] Step 2, preparation of packaging glue, the specific process is as follows:
[0096] First, take 0.8g of polyvinyl alcohol-modified lignin, 0.15g of boric acid, and 2mL of methyl acrylate, and stir at room temperature for 4h. Secondly, add 0.3g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodiphenylmethane, 0.3g of N,N,N',N'-tetraepoxypropyl-4,4'-diaminodimethylsiloxane, and 1.5g of octanoic acid oligomer to the aged solution, and continue stirring for 40min. Finally, continue to add 0.15g of nano-titanium dioxide, 0.015g of avobenzone, and 0.015g of triphenylsulfonium tetrafluoroborate, stir at room temperature for 40min to obtain encapsulation glue for use.
[0097] Step 3, UV curing of the encapsulation glue, the specific process is as follows:
[0098] The encapsulation glue was dropped onto a 1cmx1cm PTFE substrate and evenly coated at 3000r / min. The operation was repeated 5 times and finally placed into 800mJ / cm 2 After polymerization, peel off the light-cured encapsulation glue to obtain.
Claims
1. A method for preparing a biomass-based OLED electronic component encapsulation adhesive, characterized in that: The specific steps include: Step 1, preparing polyvinyl alcohol modified lignin; The specific process of step 1 is as follows: Step 1.1, taking 10g-50g of broadleaf lignin and dispersing it in 400-2000mL of ethanol / tetrahydrofuran solution and extracting it for 12h-24h to obtain extracted lignin; Step 1.2: Disperse 2 g to 5 g of the extracted lignin and 0.2 g to 0.5 g of sodium sulfonate in 50 mL to 100 mL of deionized water solution at 60 °C. o C-100 o C temperature and reflux for 12h-36h, cool to room temperature after the reaction, add HCl solution with a pH of 2-4 for acidification to obtain sulfonated lignin; Step 1.3, take 0.5g-1g of sulfonated lignin and 0.2g-0.5g of polyvinyl alcohol, add 0.01-0.02 mL of concentrated sulfuric acid and continue stirring for 12-24 hours to obtain colorless polyvinyl alcohol-modified lignin; Step 2, preparing encapsulation glue according to the polyvinyl alcohol-modified lignin prepared in step 1; The specific process of step 2 is as follows: Step 2.1, take 0.5g-1g of polyvinyl alcohol-modified lignin, 0.1g-0.2g of boric acid, and 1-3 mL of methyl acrylate, stir and age at room temperature for 3h-6h; Step 2.2, add 0.1g-0.5g of N,N,N',N'-tetracyclyl-4,4'-diaminodiphenylmethane, 0.1g-0.5g of N,N,N',N'-tetracyclyl-4,4'-diaminodimethylsiloxane, and 1-2g of octanoic acid oligomer to the solution aged in step 2.1, and continue stirring for 30-60 min; Step 2.3, add 0.1g-0.2g of nano titanium dioxide, 0.01g-0.02g of avobenzone, and 0.01g-0.02g of triphenylsulfonium tetrafluoroborate to the solution obtained in step 2.2, and stir at room temperature for 30min-60min to obtain a packaging glue; Step 3, UV curing the packaging glue prepared in step 2.
2. The method for preparing the biomass-based OLED electronic component encapsulation adhesive according to claim 1, characterized in that: In the step 1.3, the molecular weight of the polyvinyl alcohol is 1000-10000.
3. The method for preparing the biomass-based OLED electronic component encapsulation adhesive according to claim 1, characterized in that: The specific process of step 3 is as follows: The encapsulation glue prepared in step 2 was dropped onto the polytetrafluoroethylene substrate and evenly coated by spin coating. The operation was repeated 5 times and finally placed in 800mJ / cm 2 -1000 mJ / cm 2 Put it in a UV oven, and after polymerization, peel off the light-cured packaging glue to obtain it.