High entropy alloy powder, coating for brake disc and preparation method of coating
The dense coating is formed on the brake disc through high-entropy alloy powder and atmospheric plasma spraying technology, which solves the problem of insufficient wear and corrosion resistance of existing materials, and achieves a high-performance brake disc coating.
Patent Information
- Application Number
- CN202410386755.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-04-01
AI Technical Summary
Due to its low hardness, poor wear resistance and oxidation and rust, existing brake disc materials are difficult to meet the various operating conditions of modern automobile brake systems, especially in terms of wear resistance and corrosion resistance.
High-entropy alloy powder, including Al, Co, Ni, Cu and Ti, was prepared by aerosolization to obtain high-entropy alloy powder with a BCC crystal structure, and a thickness of 200 to 300 μm was formed on the brake disc by atmospheric plasma spraying technology. Coating ensures good bonding between layers and dense tissue.
It significantly improves the wear resistance and corrosion resistance of the coating, reduces the friction wear rate and corrosion depth, enhances the tensile strength and electrocatalytic properties of the coating, and is suitable for industrial production.
Smart Images

Figure CN118272713B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal coating materials and thermal spraying, and relates to a high entropy alloy powder, and in particular to a high entropy alloy powder and a coating for a brake disc and a method for preparing the coating. Background Art
[0002] The brake disc is a metal disc made of alloy steel and fixed to the wheel, rotating with the wheel. When the vehicle is driving and the brake is applied, the brake caliper clamps the brake disc to slow down or stop the vehicle. Generally, there are round holes on the brake disc, which is used to reduce weight and increase friction. There are many types of brake discs, which are characterized by thin walls and sand cores formed at the disc and the center. Different types of brake discs have differences in disc diameter, disc thickness and the gap between the two discs. The thickness and height of the disc hub are also different.
[0003] Although gray cast iron is very suitable for manufacturing brake discs, its hardness is low, about 200HV, and its wear resistance is limited. Brake discs are consumable parts in the brake system. If the brake discs are severely worn, the actual braking distance will be too different from the expected braking distance, thus affecting the driving maneuverability and safety. At present, the brake disc material in my country is mainly gray cast iron, which has low cost, high strength, durability, high melting point, and the heat energy generated by friction will not soften it easily. However, with the development of science and the advancement of technology, this traditional metal material has a single mechanical property, is easy to oxidize and rust, and has poor thermal fatigue resistance, braking performance and wear resistance. It can no longer meet the service requirements of multiple working conditions at the same time, and it is difficult to adapt to the current development of the automotive brake disc industry. Therefore, it is also urgent to upgrade the technology of the brake disc.
[0004] High entropy alloy is a new type of alloy developed in the past decade, which has four major effects: high entropy effect in thermodynamics, slow diffusion effect in kinetics, lattice mismatch effect in crystal structure and cocktail effect in performance. This type of alloy has many excellent properties such as high strength, high hardness, excellent wear resistance, corrosion resistance, low temperature resistance, high temperature oxidation resistance and tempering softening resistance.
[0005] Thermal spraying technology has its own unique advantages compared with other technologies, mainly including the following aspects: (1) There are more than ten spraying methods, which can be comprehensively selected according to factors such as performance requirements, substrate type, equipment conditions and production efficiency; (2) There are a wide variety of spraying materials, and the temperature in the high-temperature zone is high enough to spray refractory materials; (3) It has a wide range of applications and is not limited by the size of the workpiece or the site; (4) The coating thickness is controllable.
[0006] CN106756717A discloses a method for preparing a high-strength and wear-resistant copper-nickel-tin alloy coating, which specifically discloses that a Cu15Ni8SnNb coating is prepared on a stainless steel substrate by a thermal spraying method. The prepared alloy coating has better wear resistance than an alloy block of the same material, and the wear scar depth of the coating is significantly smaller than that of an alloy material of the same material. However, compared with the present invention, its wear rate is still relatively high.
[0007] Therefore, it is necessary to provide an alloy coating with better wear resistance and corrosion resistance for use in the automotive brake disc industry. Summary of the invention
[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high entropy alloy powder, a coating for a brake disc and a method for preparing the coating. The coating for a brake disc provided by the present invention has good interlayer bonding, dense structure, and excellent wear resistance and corrosion resistance.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a high entropy alloy powder, wherein raw materials for preparing the high entropy alloy powder include Al powder, Co powder, Ni powder, Cu powder and Ti powder;
[0011] The molar ratio of the metal elements Al, Co, Ni, Cu and Ti in the high entropy alloy powder is 1:1:1:1:(0.7-1.3), for example, it can be 1:1:1:1:0.7, 1:1:1:1:0.8, 1:1:1:1:0.9, 1:1:1:1:1, 1:1:1:1:1:1.1, 1:1:1:1:1.2 or 1:1:1:1:1:3, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0012] The high entropy alloy powder has a single BCC crystal structure.
[0013] As a preferred technical solution of the present invention, the particle size of the high entropy alloy powder is 25 to 75 μm, for example, it can be 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm or 75 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0014] Preferably, the purity of the Al powder, Co powder, Ni powder, Cu powder and Ti powder is ≥99.9%, for example, it can be 99.9%, 99.92%, 99.94%, 99.96%, 99.98% or 99.999%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0015] It is worth noting that the present invention uses Al powder, Co powder, Ni powder, Cu powder and Ti powder with a purity of ≥99.9% as raw materials to obtain a high entropy alloy powder with a particle size range of 25 to 75 μm, so that the high entropy alloy powder has a higher purity, and the high entropy alloy powder has a crystal structure of a BCC solid solution phase and thus has a high entropy effect, which can improve the solubility of the alloy system and the metal compound, and improve the bonding force between the alloy and the metal compound.
[0016] In a second aspect, the present invention provides a coating for a brake disc, wherein the coating for a brake disc is prepared using the high entropy alloy powder provided in the first aspect.
[0017] As a preferred technical solution of the present invention, the thickness of the brake disc coating is 200-300 μm, for example, it can be 200 μm, 220 μm, 240 μm, 260 μm, 280 μm or 300 μm, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 250-300 μm.
[0018] It is worth noting that the thickness of the coating for the brake disc of the present invention is 200-300 μm. If the coating thickness is too large, the bonding strength between the coating and the substrate will be insufficient, and it will be easy to fall off over a long period of time, which will increase the cost and reduce the competitiveness of the product. If the coating thickness is too small, the coating will be prone to cracking, falling off, etc., affecting the durability of the coating, and it will be easily corroded by corrosive media, thereby reducing the corrosion resistance of the coating. At the same time, it will be easily worn, thereby exposing the substrate and causing substrate damage.
[0019] In a third aspect, the present invention provides a method for preparing the brake disc coating provided in the second aspect, the preparation method comprising the following steps:
[0020] (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in molar ratio, and then atomized and sifted to obtain high entropy alloy powder;
[0021] (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used;
[0022] (3) Using the alloy powder to be used as a raw material, atmospheric plasma spraying is performed on the pretreated surface of the brake disc substrate to obtain the brake disc coating.
[0023] The present invention adopts a gas atomization method to prepare high entropy alloy powder with good powder sphericity, so as to ensure good fluidity of the powder during the spraying process; then an atmospheric plasma spraying method is adopted and the spraying parameters are adjusted to achieve the maximum optimization of the microscopic morphology of the brake disc coating; finally, a brake disc coating with good interlayer bonding, dense structure, and excellent wear resistance and corrosion resistance is obtained.
[0024] Furthermore, the high entropy alloy powder of the present invention has a single BCC crystal structure. After the atmospheric plasma spraying described in step (3), Ni in the alloy occupies part of the node positions of Cu atoms as a solute atom and undergoes a solid solution reaction to generate Cu 0.81 Ni 0.19 Alloy phase, obtained with Cu 0.81 Ni 0.19 The FCC (face-centered cubic) crystal structure represented by TiCo3 significantly improves the tensile strength, wear resistance, corrosion resistance, electrocatalytic performance and thermoelectric lamp performance of the coating.
[0025] As a preferred technical solution of the present invention, the gas atomization powder making in step (1) comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder until the melt drips, and then performing high-pressure atomization.
[0026] Preferably, the vacuum degree in the gas atomization powder making is 2.5×10 -4 ~3.5×10 -4 Pa, for example, can be 2.5×10 -4 Pa, 2.7×10 -4 Pa, 2.9×10 -4 Pa, 3.1×10 -4 Pa, 3.3×10 -4 Pa or 3.5×10 -4 Pa, but not limited to the listed values, other values not listed within the numerical range are also applicable.
[0027] Preferably, the smelting power is 30-40KW, for example, 30KW, 32KW, 34KW, 36KW, 38KW or 40KW, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the repeated smelting is performed 3 to 5 times, for example, 3 times, 4 times or 5 times.
[0029] Preferably, the gas used for the high-pressure atomization includes argon.
[0030] Preferably, the pressure of the high-pressure atomization is 7.5-8.5 MPa, for example, 7.5 MPa, 7.7 MPa, 7.9 MPa, 8.1 MPa, 8.3 MPa or 8.5 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] The pressure of the high-pressure atomization in the present invention is 7.5-8.5 MPa. If the pressure is too high, the gas consumption will increase, and the powder particle size will be too small, which is not conducive to spraying to form a coating. If the pressure is too low, the powder fluidity will be poor, the loose packing ratio will be small, the particle size will increase and become irregular and uneven.
[0032] As a preferred technical solution of the present invention, the temperature of the preheat treatment in step (2) is 180-230°C, for example, it can be 180°C, 190°C, 200°C, 210°C, 220°C or 230°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the preheating time in step (2) is 150 to 200 min, for example, 150 min, 160 min, 170 min, 180 min, 190 min or 200 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] As a preferred technical solution of the present invention, the pretreatment in step (3) includes: sequentially performing sandblasting pretreatment, cleaning and drying on the surface of the brake disc substrate.
[0035] Preferably, the sandblasting material used in the sandblasting pretreatment is brown corundum sand.
[0036] Preferably, the particle size of the brown corundum sand is any one of 16#, 18#, 20#, 22# or 24# or a combination of at least two thereof. Typical but non-limiting combinations include: a combination of 16# brown corundum sand and 18# brown corundum sand, a combination of 22# brown corundum sand and 24# brown corundum sand, a combination of 16# brown corundum sand, 18# brown corundum sand, 20# brown corundum sand and 24# brown corundum sand, or a combination of 16# brown corundum sand, 18# brown corundum sand, 20# brown corundum sand, 22# brown corundum sand and 24# brown corundum sand.
[0037] Preferably, the compressed air pressure in the sandblasting pretreatment is 0.3-0.8 MPa, for example, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa or 0.8 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the angle between the spray gun and the surface of the brake disc substrate in the sandblasting pretreatment is 40-50°, for example, it can be 40°, 41°, 42°, 43°, 44°, 45°, 46°, 47°, 48°, 49° or 50°, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] Preferably, the cleaning comprises cleaning with a degreasing agent.
[0040] In the pretreatment of the present invention, after the sandblasting treatment, the surface of the substrate is repeatedly purged with compressed air to make the surface clean and free of dust particles, and then the substrate is cleaned and dried with a degreasing agent to remove any residual oil stains.
[0041] Preferably, the brake disc substrate is made of cast iron.
[0042] As a preferred technical solution of the present invention, the spraying distance in the atmospheric plasma spraying in step (3) is 100 to 150 mm, for example, it can be 100 mm, 110 mm, 120 mm, 130 mm, 140 mm or 150 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] Preferably, the hydrogen flow rate of the plasma gas flow in the atmospheric plasma spraying in step (3) is 3 to 6 L / min, for example, it can be 3 L / min, 3.5 L / min, 4 L / min, 4.5 L / min, 5 L / min, 5.5 L / min or 6 L / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Preferably, the argon gas flow rate in the atmospheric plasma spraying in step (3) is 30 to 50 L / min, for example, it can be 30 L / min, 34 L / min, 38 L / min, 42 L / min, 46 L / min or 50 L / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] Preferably, the spraying current in the atmospheric plasma spraying in step (3) is 480-550A, for example, it can be 480A, 490A, 500A, 510A, 520A, 530A, 540A or 550A, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] Preferably, the spraying voltage in the atmospheric plasma spraying in step (3) is 50-60 V, for example, 50 V, 52 V, 54 V, 56 V, 58 V or 60 V, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0047] Preferably, the translation speed of the spray gun in the atmospheric plasma spraying in step (3) is 150 to 400 mm / s, for example, it can be 150 mm / s, 200 mm / s, 250 mm / s, 300 mm / s, 350 mm / s or 400 mm / s, but is not limited to the listed values, and other values not listed within the numerical range are also applicable; the translation spacing of the spray gun is 3 mm.
[0048] Preferably, the powder feeding speed in the atmospheric plasma spraying in step (3) is 2 to 10 g / min, for example, it can be 2 g / min, 3 g / min, 4 g / min, 5 g / min, 6 g / min, 7 g / min, 8 g / min, 9 g / min or 10 g / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0049] Preferably, the powder feeding method of the atmospheric plasma spraying in step (3) includes vertical jet powder feeding.
[0050] Preferably, the atmospheric plasma spraying in step (3) is repeated 4 to 6 times, for example, 4 times, 5 times or 6 times.
[0051] The selection of process parameters in the atmospheric plasma spraying process of the present invention will affect the thickness and uniformity of the obtained brake disc coating. Only by strictly controlling the spraying parameters can the microscopic morphology of the brake disc coating be optimized to the greatest extent.
[0052] As a preferred technical solution of the present invention, the method for preparing a brake disc coating provided in the second aspect of the present invention comprises the following steps:
[0053] (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in molar ratio, and then atomized and pulverized to obtain a high entropy alloy powder with a particle size of 25 to 75 μm after sieving;
[0054] The gas atomization powder making comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder with purity ≥99.9% for 3 to 5 times until the melt drips, and then using argon gas for high pressure atomization;
[0055] The vacuum degree in the gas atomization powder making is 2.5×10 -4 ~3.5×10 -4 Pa, the smelting power is 30-40KW, and the pressure of the high-pressure atomization is 7.5-8.5MPa;
[0056] (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used;
[0057] Wherein, the temperature of the preheating treatment is 180-230°C and the time is 150-200min;
[0058] (3) using the alloy powder to be used as a raw material, performing atmospheric plasma spraying on the pretreated surface of the brake disc substrate to obtain the brake disc coating with a thickness of 200 to 300 μm;
[0059] The pretreatment includes: sequentially sandblasting the surface of the cast iron brake disc substrate, cleaning and drying; the sandblasting material used in the sandblasting pretreatment includes brown corundum sand, and the compressed air pressure is 0.3-0.8 MPa; the angle between the spray gun and the surface of the brake disc substrate is 40-50°; the cleaning includes cleaning with a degreasing agent;
[0060] The spraying distance in the atmospheric plasma spraying is 100-150 mm; the hydrogen flow rate of the plasma gas flow is 3-6 L / min; the argon flow rate is 30-50 L / min; the spraying current is 480-550 A; the spraying voltage is 50-60 V; the spray gun translation speed is 150-400 mm / s, and the spray gun translation spacing is 3 mm; the powder feeding speed is 2-10 g / min; the powder feeding method includes vertical jet powder feeding; and the number of repeated passes is 4-6 times.
[0061] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0062] Compared with the prior art, the present invention has the following beneficial effects:
[0063] (1) The high entropy effect of the high entropy alloy powder provided by the present invention due to its special BCC solid solution phase crystal structure greatly improves the solubility of the alloy system and the metal compound, and improves the bonding strength between the alloy and the metal compound;
[0064] (2) The present invention adopts gas atomization to prepare high entropy alloy powder, so that the obtained powder has good sphericity and good fluidity of the powder is ensured during the spraying process;
[0065] (3) The high entropy alloy powder provided by the present invention has a diffusion hysteresis effect. In the supersaturated solid solution, a hard phase is easily precipitated and plays a role of dispersion strengthening. In addition, the precipitated hard phase is easy to form an oxidation protective glaze layer during the friction process of the coating, thereby achieving the effect of significantly improving the friction performance of the coating;
[0066] (4) The present invention adopts plasma spraying technology to prepare the coating for brake discs, which has low cost and is suitable for industrial production. The prepared coating has the characteristics of high hardness, wear resistance and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 is the XRD spectrum of the brake disc coating and high entropy alloy powder provided in Example 3 of the present invention;
[0068] Figure 2 is a cross-sectional SEM image of the coating for a brake disc provided in Example 3 of the present invention;
[0069] Figure 3 This is a SEM image of the coating surface after the friction test of the brake disc coating provided in Example 3 of the present invention;
[0070] Figure 4 This is a SEM image of the coating surface after the corrosion test of the brake disc coating provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0071] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0072] The following examples and comparative examples provide that the grinding ball in the friction and wear test of the coating is a GCr 15 steel ball, the load is 10N, the frequency is 4Hz, the wear scar length is 5m, and the total sliding distance is 100m; in the corrosion test, a CHI 604E electrochemical workstation is used to simulate the corrosion behavior of the alloy coating in seawater (3.5% NaCl solution).
[0073] Example 1
[0074] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; and the preparation method of the coating for a brake disc comprises the following steps:
[0075] (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in a molar ratio of 1:1:1:1:1:1, and then atomized to obtain a high entropy alloy powder having a particle size of 50 to 60 μm and a single BCC crystal structure after sieving;
[0076] The gas atomization powder making comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder with purity ≥ 99.9% for 4 times until the melt drips, and then using argon gas for high-pressure atomization;
[0077] The vacuum degree in the gas atomization powder making is 3×10 -4 Pa, the smelting power is 40KW, and the pressure of the high-pressure atomization is 8MPa;
[0078] (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used;
[0079] Wherein, the temperature of the preheating treatment is 200°C and the time is 180min;
[0080] (3) The pre-treated brake disc substrate surface is subjected to atmospheric plasma spraying using the alloy powder to be used as raw material to obtain a thickness of 287 μm and a hardness of 309 HV 0.1 The brake disc coating;
[0081] The pretreatment includes: sandblasting pretreatment, cleaning and drying the surface of the cast iron brake disc substrate in sequence; the sandblasting material used in the sandblasting pretreatment is 20# brown corundum sand, and the compressed air pressure is 0.5MPa; the angle between the spray gun and the surface of the brake disc substrate is 45°; the cleaning includes cleaning with a degreasing agent;
[0082] The spraying distance in the atmospheric plasma spraying is 100 mm; the hydrogen flow rate of the plasma gas flow is 6 L / min; the argon flow rate is 40 L / min; the spraying current is 519 A; the spraying voltage is 55 V; the spray gun translation speed is 200 mm / s, and the spray gun translation spacing is 3 mm; the powder feeding speed is 2.5 g / min; the powder feeding method includes vertical jet powder feeding; and the number of repeated passes is 5 times.
[0083] Example 2
[0084] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; and the preparation method of the coating for a brake disc comprises the following steps:
[0085] (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in a molar ratio of 1:1:1:1:0.7, and then atomized to obtain a high entropy alloy powder having a particle size of 30 to 70 μm and a single BCC crystal structure after sieving;
[0086] The gas atomization powder making comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder with purity ≥99.9% for 3 times until the melt drips, and then using argon gas for high-pressure atomization;
[0087] The vacuum degree in the gas atomization powder making is 3.5×10 -4 Pa, the smelting power is 40KW, and the pressure of the high-pressure atomization is 7.5MPa;
[0088] (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used;
[0089] Wherein, the temperature of the preheating treatment is 180°C and the time is 200min;
[0090] (3) The pre-treated brake disc substrate surface is subjected to atmospheric plasma spraying using the alloy powder to be used as raw material to obtain a thickness of 213 μm and a hardness of 257 HV 0.1 The brake disc coating;
[0091] The pretreatment includes: sandblasting pretreatment, cleaning and drying the surface of the cast iron brake disc substrate in sequence; the sandblasting material used in the sandblasting pretreatment is 20# brown corundum sand, and the compressed air pressure is 0.3MPa; the angle between the spray gun and the surface of the brake disc substrate is 40°; the cleaning includes cleaning with a degreasing agent;
[0092] The spraying distance in the atmospheric plasma spraying is 150 mm; the hydrogen flow rate of the plasma gas flow is 3 L / min; the argon flow rate is 50 L / min; the spraying current is 550 A; the spraying voltage is 60 V; the spray gun translation speed is 150 mm / s, and the spray gun translation spacing is 3 mm; the powder feeding speed is 2 g / min; the powder feeding method includes vertical jet powder feeding; and the number of repeated passes is 4 times.
[0093] Example 3
[0094] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; and the preparation method of the coating for a brake disc comprises the following steps:
[0095] (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in a molar ratio of 1:1:1:1:1.3, and then atomized to obtain a high entropy alloy powder having a particle size of 25 to 75 μm and a single BCC crystal structure after sieving;
[0096] The gas atomization powder making comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder with purity ≥99.9% for 5 times until the melt drips, and then using argon gas for high-pressure atomization;
[0097] The vacuum degree in the gas atomization powder making is 2.5×10 -4 Pa, the smelting power is 30KW, and the pressure of the high-pressure atomization is 8.5MPa;
[0098] (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used;
[0099] The preheating temperature is 230°C and the time is 150 min.
[0100] (3) The pre-treated brake disc substrate surface is subjected to atmospheric plasma spraying using the alloy powder to be used as raw material to obtain a thickness of 293 μm and a hardness of 321 HV 0.1 The brake disc coating;
[0101] The pretreatment includes: sandblasting pretreatment, cleaning and drying the surface of the cast iron brake disc substrate in sequence; the sandblasting material used in the sandblasting pretreatment is 20# brown corundum sand, and the compressed air pressure is 0.8MPa; the angle between the spray gun and the surface of the brake disc substrate is 50°; the cleaning includes cleaning with a degreasing agent;
[0102] The spraying distance in the atmospheric plasma spraying is 120 mm; the hydrogen flow rate of the plasma gas flow is 4.6 L / min; the argon flow rate is 30 L / min; the spraying current is 480 A; the spraying voltage is 50 V; the spray gun translation speed is 400 mm / s, and the spray gun translation spacing is 3 mm; the powder feeding speed is 10 g / min; the powder feeding method includes vertical jet powder feeding; and the number of repeated passes is 6 times.
[0103] The XRD spectra of the high entropy alloy powder and the brake disc coating provided in this embodiment are as follows: Figure 1 The cross-sectional SEM image of the brake disc coating is shown in Figure 2 shown.
[0104] The SEM images of the coating surface after the friction test and the SEM images of the coating surface after the corrosion test for the brake disc provided in this embodiment are shown in FIG. Figure 3 and Figure 4 shown.
[0105] according to Figure 3 It can be seen that after friction, the friction surface of the brake disc coating provided in this embodiment is quite smooth, accompanied by some small pits, and the wear marks are very shallow. The wear marks are difficult to distinguish from the substrate, and the wear resistance is excellent.
[0106] according to Figure 4 It can be seen that the brake disc coating provided in this embodiment has a relatively smooth surface after corrosion, less accumulation of corrosion products, only some smaller corrosion pits, fewer holes, and shallow corrosion depth, indicating that it has good corrosion resistance.
[0107] The friction and wear test and corrosion test results of the brake disc coatings provided in Examples 1-3 are shown in Table 1.
[0108] Table 1
[0109]
[0110] From the analysis of Table 1, it can be seen that the brake disc coating provided by the present invention has better wear resistance and corrosion resistance; among them, the brake disc coating provided by Example 3 has the best wear resistance and corrosion resistance.
[0111] Ⅰ. Effect of coating thickness on the performance of the coating for the brake disc
[0112] Example 4
[0113] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0114] In this embodiment, the spraying distance in the atmospheric plasma spraying in step (3) is modified to 110 mm, and the hydrogen flow rate of the plasma gas flow is modified to 3 L / min.
[0115] The thickness of the brake disc coating prepared in this embodiment is 275 μm.
[0116] Example 5
[0117] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0118] In this embodiment, the spraying distance in the atmospheric plasma spraying in step (3) is modified to 130 mm, and the hydrogen flow rate of the plasma gas flow is modified to 4 L / min.
[0119] The thickness of the brake disc coating prepared in this embodiment is 269 μm.
[0120] Example 6
[0121] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0122] In this embodiment, the spraying distance in the atmospheric plasma spraying in step (3) is modified to 150 mm, and the hydrogen flow rate of the plasma gas flow is modified to 5 L / min.
[0123] The thickness of the brake disc coating prepared in this embodiment is 253 μm.
[0124] Example 7
[0125] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0126] In this embodiment, the spraying distance in the atmospheric plasma spraying in step (3) is modified to 200 mm, and the hydrogen flow rate of the plasma gas flow is modified to 5.5 L / min.
[0127] The thickness of the brake disc coating prepared in this embodiment is 190 μm.
[0128] Example 8
[0129] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0130] In this embodiment, the spraying distance in the atmospheric plasma spraying in step (3) is modified to 95 mm, and the hydrogen flow rate of the plasma gas flow is modified to 6.5 L / min.
[0131] The thickness of the brake disc coating prepared in this embodiment is 305 μm.
[0132] The results of the friction and wear tests and corrosion tests on the brake disc coatings provided in the above-mentioned Example 3 and Examples 4-8 are shown in Table 2.
[0133] Table 2
[0134]
[0135] According to Table 2, it can be seen that when the coating thickness is between 250 and 300 μm, the brake disc coating has excellent wear resistance and corrosion resistance. Example 3 has the highest coating thickness, and the wear resistance and corrosion resistance of the coating provided by it are the best. It can be seen that the higher the coating thickness, the better the wear resistance and corrosion resistance.
[0136] However, it can be seen from the analysis of Examples 3 and 8 that when the coating thickness is too large, the wear resistance and corrosion resistance of the coating do not continue to improve. It can be seen from the analysis of Examples 6 and 7 that when the coating thickness is too small, the wear rate and self-corrosion current density increase significantly.
[0137] Therefore, the present invention needs to strictly control the thickness of the brake disc coating so that it has better wear resistance and corrosion resistance.
[0138] II. Effect of High Entropy Alloy Powder Particle Size on the Performance of the Brake Disc Coating
[0139] Example 9
[0140] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0141] In this embodiment, the particle size of the high entropy alloy powder obtained by gas atomization powder making in step (1) is modified to 80-90 μm.
[0142] Example 10
[0143] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0144] In this embodiment, the particle size of the high entropy alloy powder obtained by gas atomization powder making in step (1) is modified to 25-40 μm.
[0145] Embodiment 11
[0146] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0147] In this embodiment, the particle size of the high entropy alloy powder obtained by gas atomization powder making in step (1) is modified to ≤10 μm.
[0148] The results of the friction and wear tests and corrosion tests on the brake disc coatings provided in the above-mentioned Example 3 and Examples 9-11 are shown in Table 3.
[0149] Table 3
[0150]
[0151]
[0152] From the analysis of Table 3, it can be seen that the particle size selection of the high entropy alloy powder in the preparation method provided by the present invention will affect the wear resistance and corrosion resistance of the coating for the brake disc;
[0153] It can be seen from the analysis of Example 3 and Example 9 that when the particle size of the selected high entropy alloy powder is too large, the wear resistance and corrosion resistance of the brake disc coating are reduced; it can be seen from the analysis of Example 3 and Example 10 that when the particle size of the selected high entropy alloy powder is further reduced, the wear resistance and corrosion resistance are slightly improved, and the wear rate, self-corrosion current density and self-corrosion potential change less. This is because the raw material powder with a finer particle size has a higher speed and temperature during the spraying process, resulting in a stronger coating density, a smaller surface porosity, fewer boundary defects, and better wear resistance. However, if the raw material size is too small (such as Example 11), the fracture toughness of the coating may be affected, and the smaller the particle size, the more complicated the powder making process, and the higher the cost, so a suitable particle size is selected to make its comprehensive performance better.
[0154] III. Influence of the process on the performance of the coating for the brake disc
[0155] Example 12
[0156] This embodiment provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Embodiment 3 only in that:
[0157] In this embodiment, the gas atomization powder preparation in step (1) is modified into a ball milling and mechanical alloying process performed sequentially.
[0158] The results of the friction and wear tests and corrosion tests on the brake disc coatings provided in Examples 3 and 12 are shown in Table 4.
[0159] Table 4
[0160]
[0161] From the analysis of Table 4, it can be seen that compared with Example 3, the wear resistance and corrosion resistance of the coating provided in Example 12 are reduced. It can be seen that the aerosol powder preparation provided by the present invention can better ensure the fluidity of the powder during the spraying process, thereby ensuring the uniformity of the coating and the bonding strength with the metal compound, so as to achieve the purpose of improving the wear resistance and corrosion resistance of the coating.
[0162] IV. Effect of the element ratio of high entropy alloy powder on the performance of the coating for the brake disc
[0163] Comparative Example 1
[0164] This comparative example provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Example 3 only in that:
[0165] In this comparative example, the molar ratio of the metal elements Al, Co, Ni, Cu and Ti in the high entropy alloy powder of step (1) is modified to 1:1:1:1:0.5.
[0166] Comparative Example 2
[0167] This comparative example provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Example 3 only in that:
[0168] In this comparative example, the molar ratio of the metal elements Al, Co, Ni, Cu and Ti in the high entropy alloy powder of step (1) is modified to 1:1:1:1:1.5.
[0169] The results of the friction and wear tests and corrosion tests on the brake disc coatings provided in Example 3 and Comparative Examples 1-2 are shown in Table 5.
[0170] Table 5
[0171]
[0172] The molar ratio of metal elements in the alloy powders provided in Comparative Examples 1 and 2 cannot meet the requirements of high entropy. The Ti powder content in the alloy powder provided in Comparative Example 1 is significantly reduced. Compared with Example 3, its corrosion resistance is improved, but its wear resistance is also significantly reduced.
[0173] The Ti powder content in the alloy powder provided in Comparative Example 2 is significantly increased, and compared with Example 3, its wear resistance and corrosion resistance are reduced (its self-corrosion potential is only 85% of the coating described in Example 3).
[0174] Therefore, the present invention needs to strictly control the content of each metal element in the high entropy alloy powder so that the coating for the brake disc has better wear resistance and corrosion resistance.
[0175] V. Effect of the Type of High Entropy Alloy Powder on the Performance of the Brake Disc Coating
[0176] Comparative Example 3
[0177] This comparative example provides a brake disc coating, wherein the raw material for preparing the brake disc coating is high entropy alloy powder; the preparation method of the brake disc coating is different from that of Example 3 only in that:
[0178] In this comparative example, the raw materials of the high entropy alloy powder in step (1) are modified to Al powder, Co powder, Ni powder, Cu powder, Ti powder and Zr powder, and the molar ratio of the metal elements Al, Co, Ni, Cu, Ti and Zr is 1:1:1:1:1:1:1.
[0179] Comparative Example 4
[0180] This comparative example provides a brake disc coating, wherein the raw material for preparing the brake disc coating is high entropy alloy powder; the preparation method of the brake disc coating is different from that of Example 3 only in that:
[0181] In this comparative example, the raw materials of the high entropy alloy powder in step (1) are modified to Al powder, Co powder, Ni powder, Cr powder, Ti powder and Si powder, and the molar ratio of the metal elements Al, Co, Ni, Cr, Ti and Si is 1:1:1:1:1:1:1.
[0182] Comparative Example 5
[0183] This comparative example provides a brake disc coating, wherein the raw material for preparing the brake disc coating is high entropy alloy powder; the preparation method of the brake disc coating is different from that of Example 3 only in that:
[0184] In this comparative example, the raw materials of the high entropy alloy powder in step (1) are modified to Al powder, Co powder, Ni powder and Cu powder, and the molar ratio of the metal elements Al, Co, Ni and Cu is 1:1:1:1.
[0185] Comparative Example 6
[0186] This comparative example provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Example 3 only in that:
[0187] In this comparative example, the raw materials of the high entropy alloy powder in step (1) are modified to Al powder, Co powder, Ni powder, Cu powder and Cr powder, and the molar ratio of the metal elements Al, Co, Ni, Cu and Cr is 1:1:1:1:1.
[0188] Comparative Example 7
[0189] This comparative example provides a coating for a brake disc, wherein the raw material for preparing the coating for a brake disc is high entropy alloy powder; the preparation method of the coating for a brake disc is different from that of Example 3 only in that:
[0190] In this comparative example, the raw materials of the high entropy alloy powder in step (1) are modified to Al powder, Co powder, Ni powder, Cu powder, Ti powder and Cr powder, and the molar ratio of the metal elements Al, Co, Ni, Cu, Ti and Cr is 1:1:1:1:1:1.
[0191] The results of friction and wear tests and corrosion tests on the brake disc coatings provided in Example 3 and Comparative Examples 3-7 are shown in Table 6.
[0192] Table 6
[0193]
[0194]
[0195] Compared with Example 3, the high entropy alloy powder provided in Comparative Example 3 adds Zr powder. The addition of Zr powder will slightly improve the wear resistance of the alloy coating, but will cause the corrosion resistance of the coating to be significantly reduced (the corrosion test results show that the surface self-corrosion current density is 1.5 times that of the coating described in Example 3, and the self-corrosion potential is only 4 / 5 of that of the coating described in Example 3);
[0196] Compared with Example 3, the high entropy alloy powder provided in Comparative Example 4 adds Si powder. The increase of Si powder makes its wear rate slightly lower than that of Example 3, but its corrosion test results show that the surface self-corrosion current density is 1.5 times that of the coating described in Example 3, and the self-corrosion potential is only 4 / 5 of that of the coating described in Example 3. The corrosion resistance is quite different from that of Example 3.
[0197] Compared with Example 3, the high entropy alloy powder provided in Comparative Example 5 lacks Ti powder. Metal Ti has properties such as high strength and corrosion resistance. The lack of Ti powder will cause the wear resistance and corrosion resistance of the alloy to be greatly reduced.
[0198] Compared with Example 3, the high entropy alloy powder provided in Comparative Example 6 replaces Ti powder with Cr powder. Compared with Comparative Example 5, its wear resistance and corrosion resistance are improved, but the addition of Cr powder does not achieve the effect of adding Ti powder, indicating that adding Ti powder is more helpful to obtain the wear resistance and corrosion resistance of the alloy described in the present invention.
[0199] Compared with Example 3, Cr powder is added to the high entropy alloy powder provided in Comparative Example 7. It is known to those skilled in the art that metal Cr has excellent corrosion resistance. However, analysis of Example 3 and Comparative Example 7 shows that the corrosion resistance of the brake disc coating obtained by adding Cr powder with higher corrosion resistance does not reach the effect of Example 3, indicating that the addition of Cr powder will affect the corrosion resistance of the brake disc coating.
[0200] Therefore, the present invention needs to strictly control the types of elements in the high entropy alloy powder so that the coating for the brake disc has better wear resistance and corrosion resistance.
[0201] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A coating for a brake disc, characterized in that: The brake disc coating is prepared by using high entropy alloy powder; the raw materials for preparing the high entropy alloy powder are composed of Al powder, Co powder, Ni powder, Cu powder and Ti powder; The molar ratio of the metal elements Al, Co, Ni, Cu and Ti in the high entropy alloy powder is 1:1:1:1:(1.1-1.3); The high entropy alloy powder has a single BCC crystal structure.
2. The brake disc coating according to claim 1, characterized in that: The particle size of the high entropy alloy powder is 25-75 mm.
3. The brake disc coating according to claim 1, characterized in that: The purity of the Al powder, Co powder, Ni powder, Cu powder and Ti powder is ≥99.9%.
4. The brake disc coating according to claim 1, characterized in that: The thickness of the brake disc coating is 200-300 mm.
5. The brake disc coating according to claim 4, characterized in that: The thickness of the brake disc coating is 250-300 mm.
6. A method for preparing a brake disc coating according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in molar ratio, and then atomized and pulverized to obtain high entropy alloy powder after sieving; (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used; (3) Using the alloy powder to be used as a raw material, atmospheric plasma spraying is performed on the pretreated surface of the brake disc substrate to obtain the brake disc coating.
7. The preparation method according to claim 6, characterized in that: The gas atomization powder making in step (1) comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder until the melt drips, and then performing high-pressure atomization.
8. The preparation method according to claim 7, characterized in that: The vacuum degree in the gas atomization powder making is 2.5×10 -4 ~3.5×10 -4 Pa.
9. The preparation method according to claim 7, characterized in that: The smelting power is 30-40 kW.
10. The preparation method according to claim 7, characterized in that: The number of repeated smelting is 3 to 5 times.
11. The preparation method according to claim 7, characterized in that: The gas used for the high-pressure atomization includes argon.
12. The preparation method according to claim 7, characterized in that: The pressure of the high-pressure atomization is 7.5-8.5 MPa.
13. The preparation method according to claim 6, characterized in that: The temperature of the preheating treatment in step (2) is 180-230°C.
14. The preparation method according to claim 6, characterized in that: The preheating time in step (2) is 150 to 200 minutes.
15. The preparation method according to claim 6, characterized in that: The pretreatment in step (3) includes: sequentially performing sandblasting pretreatment, cleaning and drying on the surface of the brake disc substrate.
16. The preparation method according to claim 15, characterized in that: The sandblasting material used in the sandblasting pretreatment includes brown corundum sand.
17. The preparation method according to claim 16, characterized in that: The particle size of the brown corundum sand is any one of 16#, 18#, 20#, 22# or 24#, or a combination of at least two of them.
18. The preparation method according to claim 15, characterized in that: The compressed air pressure in the sandblasting pretreatment is 0.3-0.8 MPa.
19. The preparation method according to claim 15, characterized in that: In the sandblasting pretreatment, the angle between the spray gun and the surface of the brake disc substrate is 40-50°.
20. The preparation method according to claim 15, characterized in that: The cleaning includes cleaning with a degreasing agent.
21. The preparation method according to claim 6, characterized in that: The brake disc substrate is made of cast iron.
22. The preparation method according to claim 6, characterized in that: The spraying distance in the atmospheric plasma spraying in step (3) is 100-150 mm.
23. The preparation method according to claim 6, characterized in that: The hydrogen flow rate of the plasma gas flow in the atmospheric plasma spraying in step (3) is 3-6 L / min.
24. The preparation method according to claim 6, characterized in that: The argon gas flow rate in the atmospheric plasma spraying in step (3) is 30-50 L / min.
25. The preparation method according to claim 6, characterized in that: The spraying current in the atmospheric plasma spraying in step (3) is 480~550A.
26. The preparation method according to claim 6, characterized in that: The spraying voltage in the atmospheric plasma spraying in step (3) is 50-60V.
27. The preparation method according to claim 6, characterized in that: In the atmospheric plasma spraying in step (3), the spray gun translation speed is 150-400 mm / s, and the spray gun translation interval is 3 mm.
28. The preparation method according to claim 6, characterized in that: The powder feeding speed in the atmospheric plasma spraying in step (3) is 2-10 g / min.
29. The preparation method according to claim 6, characterized in that: The powder feeding method of the atmospheric plasma spraying in step (3) includes vertical jet powder feeding.
30. The preparation method according to claim 6, characterized in that: The atmospheric plasma spraying in step (3) is repeated 4 to 6 times.
31. The preparation method according to claim 6, characterized in that: The preparation method comprises the following steps: (1) Al powder, Co powder, Ni powder, Cu powder and Ti powder are mixed in molar ratio, and then atomized and pulverized to obtain high entropy alloy powder with a particle size of 25-75 mm after sieving; The gas atomization powder making comprises: under the protection of inert gas, repeatedly smelting Al powder, Co powder, Ni powder, Cu powder and Ti powder with purity ≥99.9% for 3 to 5 times until the melt drips, and then using argon gas for high pressure atomization; The vacuum degree in the gas atomization powder making is 2.5×10 -4 ~3.5×10 -4 Pa, the smelting power is 30-40 kW, and the pressure of the high-pressure atomization is 7.5-8.5 MPa; (2) preheating the high entropy alloy powder obtained in step (1) to obtain an alloy powder to be used; Wherein, the temperature of the preheating treatment is 180-230°C and the time is 150-200min; (3) using the alloy powder to be used as a raw material, performing atmospheric plasma spraying on the pretreated surface of the brake disc substrate to obtain the brake disc coating with a thickness of 200 to 300 mm; The pretreatment includes: sequentially performing sandblasting pretreatment, cleaning and drying on the surface of the cast iron brake disc substrate; the sandblasting material used in the sandblasting pretreatment includes brown corundum sand, and the compressed air pressure is 0.3-0.8 MPa; the angle between the spray gun and the surface of the brake disc substrate is 40-50°; the cleaning includes cleaning with a degreasing agent; The spraying distance in the atmospheric plasma spraying is 100-150 mm; the hydrogen flow rate of the plasma gas flow is 3-6 L / min; the argon flow rate is 30-50 L / min; the spraying current is 480-550 A; the spraying voltage is 50-60 V; the spray gun translation speed is 150-400 mm / s, and the spray gun translation spacing is 3 mm; the powder feeding speed is 2-10 g / min; the powder feeding method includes vertical jet powder feeding; and the number of repeated passes is 4-6 times.
Citation Information
Patent Citations
Preparing method of high-strength and wear-resistant Cu-Ni-Sn alloy coating
CN106756717A
Manufacturing method of high entropy alloy coating
TWI674334B