A whisker-reinforced UHV disc-shaped suspension porcelain insulator and a preparation method thereof

By using a specific ratio of alumina and silicon source materials, combined with the modification treatment of silicide wood powder, a whisker-enhanced mullite structure is formed, which solves the problem of degradation of the insulation performance of traditional porcelain insulators in ultra-high voltage environments, and is significantly Improves the mechanical and electrical properties of the porcelain body.

CN118290123BActive Publication Date: 2024-12-03PINGXIANG BEST INSULATOR GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410401289.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-12-03
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

Traditional porcelain insulators are prone to problems such as degradation of insulation performance and weakening of mechanical properties after long-term operation, especially in ultra-high voltage power grid environments.

Method used

Using alumina micro powder, spherical soil, feldspar, Fujian mud, rosystone, ash, quartz and other materials, combined with silicified wood powder, crystals are formed through wet ball milling, vacuum extrusion and gas drawer kiln firing. Mullite structure that must be enhanced to improve the bending strength and electrical properties of the porcelain body.

Benefits of technology

It significantly improves the bending strength and electrical performance of the porcelain body, enhances the stability and reliability of the insulator, reduces the appearance of defects such as pores, cracks and spots, and meets the performance requirements of the ultra-high voltage power grid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118290123B_ABST
    Figure CN118290123B_ABST
Patent Text Reader

Abstract

The invention discloses a whisker-reinforced UHV disc-shaped suspension porcelain insulator in the field of porcelain insulators and a preparation method thereof. The raw materials include 26-35wt% alumina micropowder, 15-20wt% ball clay, 14-19wt% feldspar, 10-15wt% Fujian mud, 6-12wt% andalusite, 6-12wt% ash soil, and 6-9wt% quartz. The steps include: wet ball milling to obtain a mixed abrasive after mixing the raw materials; sieving the mixed abrasive to remove iron, squeezing mud to obtain a mud cake and aging; extruding the mud cake to obtain a blank; using an aluminum mold cloth lining pressure to make a blank, wet spinning the blank into a green blank, drying it, and glazing, sanding, firing, and inspecting the green blank. The invention introduces andalusite and ash soil as high-aluminum raw materials and silicon sources, promotes the in-situ uniform growth of mullite whiskers, greatly improves the bending strength of the porcelain body, improves the mechanical and electrical properties of the disc-shaped suspension porcelain insulator products, and enhances stability and reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of porcelain insulators, and in particular to a whisker-reinforced ultra-high voltage disc-shaped suspension porcelain insulator and a preparation method thereof. Background Art

[0002] In power transmission and distribution systems, insulators are key components to ensure the safe operation of power equipment. Traditional porcelain insulators are usually made of materials such as glass, ceramic or rubber. However, these traditional materials have problems such as low mechanical strength and poor arc resistance. In recent years, in order to overcome these limitations, large-tonnage disc suspension porcelain insulators have emerged as a new type of insulator with higher electromechanical performance.

[0003] Large-tonnage disc-shaped suspension porcelain insulators are mainly composed of four parts, namely, the ceramic body, steel cap, steel foot, and connection hardware, among which the ceramic body is the main insulating component. The manufacturing process of ordinary porcelain insulators generally uses bauxite, feldspar, quartz and clay as the main raw materials. The composition of the raw materials is complex and the impurity content is high. The produced porcelain body is prone to defects such as pores, rust spots, and pinholes. Therefore, the strength of the porcelain body is generally low, and accidents such as cracking, glaze cracking and electrical breakdown are prone to occur during operation. In addition, due to the large differences in thermal properties of components made of different materials, the expansion coefficients when heated are different. When the temperature of the external environment changes greatly, the extension and contraction of each material are uneven, and a large axial compressive stress and tangential shear stress are generated inside the porcelain insulation. When the insulators in operation are subjected to strong electric fields, ice coating, and mechanical stresses accumulated to a certain extent for a long time, microcracks will occur in the insulation parts, which may develop into fractures when superimposed with external forces, and the insulation performance will decrease to become low-value and zero-value insulators.

[0004] Therefore, with the rapid construction and development of UHV power grids at home and abroad, there is an urgent need to develop a large-tonnage disc-shaped suspension porcelain insulator with higher strength and superior electromechanical properties for use in UHV transmission lines. Summary of the invention

[0005] The object of the present invention is to provide a whisker-reinforced UHV disc-shaped suspension porcelain insulator and a preparation method thereof, which solves the problems of reduced insulation performance and weakened mechanical properties of existing disc-shaped suspension porcelain insulators after long-term operation.

[0006] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0007] A whisker-reinforced UHV disc-shaped suspension porcelain insulator, the raw materials of which include: 26-35wt% alumina powder, 15-20wt% ball clay, 14-19wt% feldspar, 10-15wt% Fujian mud, 6-12wt% andalusite, 6-12wt% ash soil and 6-9wt% quartz.

[0008] A further improvement is that the mass ratio of the andalusite to the ash soil is 1:1.

[0009] A further improvement is that the Al2O3 content in the andalusite and ash soil is greater than 55wt%.

[0010] A further improvement is that the raw material of the porcelain insulator also includes: 0.2-2wt% of silicified wood powder.

[0011] A further improvement is that the petrified wood powder is white petrified wood powder modified by calcium acetate and aluminum sulfate.

[0012] The present invention also provides a method for preparing a whisker-reinforced UHV disc-shaped suspension porcelain insulator, the steps comprising:

[0013] S1, mixing alumina powder, ball clay, feldspar, Fujian mud, andalusite, ash soil, and quartz in proportion and then wet-milling to obtain a mixed abrasive;

[0014] S2, screening the mixed abrasive to remove iron, and then squeezing mud to obtain mud cake and aging it;

[0015] S3, extruding the mud cake in a vacuum mud kneading machine to obtain a blank;

[0016] S4, using an aluminum mold cloth lining pressure to make a blank, wet spinning the blank into shape, and drying to obtain a green blank;

[0017] S5. After glazing, sanding, firing and inspecting the green body, the whisker-reinforced UHV disc-shaped suspension porcelain insulator with in-situ generated mullite is obtained.

[0018] A further improvement is that in step S1, during wet ball milling, the mass ratio of the blank particles, water and balls is 1:1:2, and the ball milling time is 30-35 hours;

[0019] In step S2, the sieving and impurity removal is 3 passes of high-strength slurry sieving, the iron removal is 3 passes of high-strength slurry iron removal, the mud fineness in the mud squeezing process is 0.1% to 0.2% of the 325 mesh sieve residue, the aging time is 80-100h, the aging chamber temperature is 15-30°C, and the aging chamber humidity is 75%;

[0020] In step S3, the moisture difference of the mud sections put into the mud mixer during extrusion is ≤0.5%, and the relative vacuum degree of the vacuum mud mixer is ≥96%;

[0021] In step S4, the moisture content of the wet spinning molding is 17.3% to 17.8%, the drying temperature is 40 to 60° C., and the drying time is 100 to 130 hours;

[0022] In step S5, the gas supply pressure of the burning gas is 6-7KPa, the gas working pressure is ≥1.5KPa, the burning temperature is 1280±10℃, and the burning time is 75m 3 Gas drawer kiln 48h, or 180m 3 Gas drawer kiln 39h.

[0023] A further improvement is that in step S1, white siliconized wood powder is added to the mixed abrasive in proportion.

[0024] A further improvement is that the preparation method of the white silicified wood powder is as follows: the white silicified wood is crushed and ground to obtain a powder, and then the powder is added to deionized water accounting for 400% to 500% of its mass under stirring conditions of 100 to 300 r / min and stirred and dispersed to obtain a powder suspension; calcium acetate solution is added to the powder suspension, the pH value is adjusted to 9.0 to 9.5, and then aluminum sulfate solution is added to the powder suspension under stirring conditions of 200 to 350 r / min, and then reacted at a temperature of 70 to 90°C and stirring conditions of 200 to 300 r / min for 3-4 hours, and finally cooled to room temperature, filtered, washed, and dried.

[0025] A further improvement is that the concentration of the calcium acetate solution is 1-3 mol / L, and the amount added is 5-10% of the mass of the powder, and the concentration of the aluminum sulfate solution is 0.5-1.2 mol / L, and the amount added is 10-20% of the mass of the powder.

[0026] The beneficial effects of the present invention are:

[0027] (1) The present invention introduces andalusite and ash soil as high-aluminum raw materials and silicon sources. The impurity content is low and they are easily decomposed into active silicon oxide and aluminum oxide at high temperatures. The two are used in combination in a specific ratio and fired in a gas drawer kiln with an isothermal and high-speed nozzle, which promotes the in-situ uniform growth of mullite whiskers. The morphology is more uniform and the aspect ratio is higher. The mullite whiskers form an interwoven network structure with the alumina block, which greatly improves the bending strength of the porcelain body, thereby effectively improving the mechanical and electrical properties of the UHV disc suspension porcelain insulator products and enhancing the stability and reliability.

[0028] (2) The present invention also introduces silicified wood powder as a silicon source in the preferred scheme, especially white silicified wood powder modified with calcium acetate and aluminum sulfate. After modification, the fluidity and bonding properties are better, while reducing the influence of non-ideal components (such as CaO, Fe2O3, etc.), avoiding the occurrence of defects such as pores, cracks, and spots on the grain boundaries of the porcelain body, thereby further improving the bending strength of the porcelain body and improving the glossiness. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1This is a microstructure diagram of a large-tonnage disc-shaped suspension porcelain insulator prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0030] The present application is further described in detail below in conjunction with the accompanying drawings. It is necessary to point out here that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0031] 1. Main raw materials:

[0032] Alumina powder: Purity requirements: Al2O3 content greater than 99wt%, α-Al2O3 conversion rate greater than 97%, true specific gravity greater than 3.90g / cm 3 , pH value is 9-11, particle size D50 is 2-10 μm, and 60-70% of the alumina powder are flaky particles, and the rest are spherical particles.

[0033] Andalusite: The main chemical components include Al2O3 58.58%, SiO2 34.80%, and its density is 3.20~3.65g / cm 3 .

[0034] Manchurian ash soil: The main chemical components include SiO2 55.35%, Al2O3 29.45%, F2O3 2.23%, TiO20.76%, loss on ignition 10.61%, FeO content less than 0.25%, and the total amount of alkali metals and alkaline earth metals less than 2.8%.

[0035] Petrified wood: purchased from Lianyungang Xiukuang Crafts Co., Ltd., the main chemical composition is SiO2, Al2O3, CaO, Fe2O3 and MgO, etc.

[0036] The remaining raw materials are conventional products with no special requirements and are all obtained through commercial channels.

[0037] 2. Specific implementation of the experiment:

[0038] Example 1

[0039] A whisker-reinforced UHV disc-shaped suspension porcelain insulator, the raw materials of which include: 26wt% alumina powder, 20wt% ball clay, 14wt% feldspar, 10wt% Fujian mud, 12wt% andalusite, 12wt% ash soil and 6wt% quartz.

[0040] Its preparation method is:

[0041] S1. Alumina powder, ball clay, feldspar, Fujian mud, andalusite, ash soil, and quartz are mixed in proportion, and the mass ratio of the mixed blank particles, water, and balls is 1:1:2, and wet ball milling is performed for 30 hours to obtain a mixed abrasive;

[0042] S2, the mixed abrasive is screened and iron removed, and the screening and impurity removal is 3 passes of high-strength slurry screening, and the iron removal is 3 passes of high-strength slurry iron removal, and then the mud is squeezed to obtain a mud cake and aged. During the mud squeezing process, the mud fineness is 0.1% of the 325 mesh sieve residue, the aging time is 80h, the aging chamber temperature is 15°C, and the aging chamber humidity is 75%;

[0043] S3, the mud cake is extruded in a vacuum mud mixer to obtain a blank, the moisture difference between the inside and outside of the mud section put into the mud mixer is 0.5%, and the relative vacuum degree of the vacuum mud mixer is 96%;

[0044] S4, using aluminum mold cloth lining pressure to make a blank, wet spinning blank forming, drying to obtain a green blank, and the wet spinning blank forming moisture content is 17.3%, the drying temperature is 40 ° C, and the drying time is 100 hours;

[0045] S5. After glazing, sanding, firing and testing the green body, the whisker-reinforced UHV disc-shaped suspension porcelain insulator with in-situ mullite is obtained. The fired gas supply pressure is 6KPa, the gas working pressure is 1.5KPa, the firing temperature is 1280℃, and the firing time is 75m. 3 Gas drawer kiln 48h.

[0046] Example 2

[0047] A whisker-reinforced UHV disc-shaped suspension porcelain insulator, the raw materials of which include: 35wt% alumina powder, 15wt% ball clay, 19wt% feldspar, 10wt% Fujian mud, 6wt% andalusite, 6wt% ash soil and 9wt% quartz.

[0048] Its preparation method is:

[0049] S1. Alumina powder, ball clay, feldspar, Fujian mud, andalusite, ash soil, and quartz are mixed in proportion, and the mass ratio of the mixed blank particles, water, and balls is 1:1:2, and wet ball milling is performed for 35 hours to obtain a mixed abrasive;

[0050] S2, the mixed abrasive is screened and iron removed, and the screening and impurity removal is 3 passes of high-strength slurry screening, and the iron removal is 3 passes of high-strength slurry iron removal, and then the mud is squeezed to obtain a mud cake and aged. During the mud squeezing process, the mud fineness is 0.2% of the 325 mesh sieve residue, the aging time is 100h, the aging chamber temperature is 30°C, and the aging chamber humidity is 75%;

[0051] S3, extruding the mud cake in a vacuum mud mixer to obtain a blank, the difference in moisture inside and outside the mud section of the mud mixer is 0.3%, and the relative vacuum degree of the vacuum mud mixer is 96.5%;

[0052] S4, using aluminum mold cloth lining pressure to make a blank, wet spinning blank forming, drying to obtain a green blank, and the wet spinning blank forming molding moisture is 17.8%, the drying temperature is 60 ° C, and the drying time is 130 hours;

[0053] S5. After glazing, sanding, firing and testing the green body, the whisker-reinforced UHV disc-shaped suspension porcelain insulator with in-situ mullite is obtained. The fired gas supply pressure is 7KPa, the gas working pressure is 1.6KPa, the firing temperature is 1290℃, and the firing time is 180m. 3 Gas drawer kiln 39h.

[0054] Example 3

[0055] A whisker-reinforced UHV disc-shaped suspension porcelain insulator, the raw materials of which include: 30wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil and 6wt% quartz.

[0056] Its preparation method is:

[0057] S1. Alumina powder, ball clay, feldspar, Fujian mud, andalusite, ash soil, and quartz are mixed in proportion, and the mass ratio of the mixed blank particles, water, and balls is 1:1:2, and wet ball milling is performed for 32 hours to obtain a mixed abrasive;

[0058] S2, the mixed abrasive is screened and iron removed, and the screening and impurity removal is 3 passes of high-strength slurry screening, and the iron removal is 3 passes of high-strength slurry iron removal, and then the mud is squeezed to obtain a mud cake and aged. During the mud squeezing process, the mud fineness is 0.15% of the 325 mesh sieve residue, the aging time is 90h, the aging chamber temperature is 25°C, and the aging chamber humidity is 75%;

[0059] S3, extruding the mud cake in a vacuum mud mixer to obtain a blank, the moisture difference between the inside and outside of the mud section in the mud mixer is 0.5%, and the relative vacuum degree of the vacuum mud mixer is 96%;

[0060] S4, using aluminum mold cloth lining pressure to make a blank, wet spinning blank forming, drying to obtain a green blank, and the wet spinning blank forming moisture content is 17.5%, the drying temperature is 50 ° C, and the drying time is 120 hours;

[0061] S5. After glazing, sanding, firing and testing the green body, the whisker-reinforced UHV disc-shaped suspension porcelain insulator with in-situ mullite is obtained. The fired gas supply pressure is 6.5 KPa, the gas working pressure is 1.6 KPa, the firing temperature is 1285°C, and the firing time is 75 m. 3 Gas drawer kiln 48h.

[0062] See also Figure 1 The whisker-reinforced UHV disc-shaped suspension porcelain insulator prepared in Example 3 of the present invention contains a large amount of in-situ generated mullite whiskers, and the main crystal phase of the porcelain insulator is an interwoven structure formed by mullite and corundum.

[0063] The UHV disc-shaped suspension porcelain insulators prepared in Example 3 were sampled and tested by the National Insulator Arrester Quality Supervision and Inspection Center. The main indicators of the test results are shown in Table 1:

[0064] Table 1: Test results of the National Insulator Arrester Quality Supervision and Inspection Center

[0065]

[0066] 3. Example Crystalline Phase Composition and Performance Testing

[0067] The porcelain insulator samples prepared in Examples 1-3 were respectively taken and subjected to the following tests:

[0068] (1) Crystalline phase composition: The phase analysis of porcelain insulator samples was performed using a PHILIPS X'Pert 30X XRD diffractometer (Cu target);

[0069] (2) Bulk density and porosity: The Archimedes drainage method was used to determine the bulk density and porosity of the porcelain insulator sample. The specific calculation formula is as follows:

[0070]

[0071]

[0072] Where ρ is the volume density, Ap is the porosity, and ρ1 is the medium density (usually distilled water is used, with a density of 1000 kg / m 3 ), m0 is the mass of the dry porcelain insulator sample in the air (g), m1 is the apparent mass of the porcelain insulator sample in water after sufficient water absorption, and m2 is the mass of the porcelain insulator sample in the air after sufficient water absorption;

[0073] (3) Bending strength: The porcelain insulator samples were processed into 25 mm × 25 mm × 150 mm specimens. The samples were loaded with a WHY-200 fully automatic flexural testing machine at a loading rate of 0.05 KN / s. The maximum load was recorded and the bending strength was calculated. The specific calculation formula is as follows:

[0074]

[0075] In the formula, F max is the maximum pressure value, L s is the distance between the lower blades, b and h are the width and height of the porcelain insulator sample, respectively.

[0076] The test results are summarized in Table 2:

[0077] Table 2: Crystalline phase composition and performance test results of each embodiment

[0078] Example 1 Example 2 Example 3 Bending strength MPa 175 177 182 <![CDATA[Bulk density g / cm 3 > 2.76 2.76 2.77 Porosity% 4.1 4.03 3.2 Mullite wt% 8.18 9.11 11.88 Corundum phase wt% 29.22 27.54 29.03 Quartz wt% 5.04 4.31 3.04 Glass phase wt% 53.46 55.01 52.85

[0079] Referring to Table 2, it can be seen that the porcelain insulators prepared in Examples 1-3 of the present invention have a bending strength greater than 175 MPa and a volume density greater than 2.76 g / cm 3 , and the porosity is lower than 4.1%, and all indicators can meet the requirements of UHV power grid.

[0080] 4. Experiment on the influence of the dosage of andalusite and ash soil on the crystal phase composition and performance

[0081] On the basis of Example 3, the dosage ratio was adjusted with reference to Table 3 below to form different comparative examples, in which the contents of other components in each comparative example were kept unchanged, and only the dosage ratio of andalusite and ash soil was adjusted, and each comparative example adopted the same preparation method as Example 3.

[0082] Table 3: Dosages of andalusite and ash soil in each comparative example

[0083]

[0084]

[0085] According to the same detection method as in (III) above, the crystal phase composition and performance of the porcelain insulator samples prepared in Comparative Examples 1-10 were tested, and the test results were statistically obtained in the following Table 4:

[0086] Table 4: Crystalline phase composition and performance test results of comparative examples 1-10

[0087]

[0088]

[0089] It can be seen from Table 4 above that the change in the amount of andalusite and ash soil will cause the bending strength of mullite to show obvious regular changes, and the volume density and porosity also basically show regular changes (except for a few comparative examples), that is: as the amount ratio of andalusite and ash soil is closer to 1:1, its bending strength is higher, the volume density is higher, the porosity is correspondingly smaller, and the overall performance is better. Moreover, even when the amount of andalusite and ash soil is very close to 1:1, such as comparative examples 5 and 6, there is a certain gap between the bending strength, volume density, and porosity data and the data of Example 3 of the present invention, which shows that when the amount of andalusite and ash soil is 1:1, the performance of the porcelain insulator will be significantly improved. In addition, when the amount of andalusite and ash soil is within the range of 6-12wt%, its bending strength, volume density, and porosity are also improved to a certain extent compared with the comparative examples outside this range.

[0090] 5. Experiment on the effect of adding siliconized wood powder on performance

[0091] The petrified wood raw materials were divided into three categories according to their colors: white petrified wood, brown petrified wood, and reddish-brown petrified wood. Their main chemical components were analyzed, and the analysis results were statistically obtained in Table 5 below.

[0092] Table 5: Main chemical components of different petrified wood raw materials

[0093]

[0094] Using the above petrified wood raw material, on the basis of Example 3, the following comparative example was set up:

[0095] Comparative Example 11

[0096] A whisker-reinforced UHV disc suspension porcelain insulator, the raw materials of which include: 29.8wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil, 6wt% quartz, and 0.2wt% petrified wood powder. The preparation method is the same as that of Example 3.

[0097] The silicified wood powder is a white silicified wood powder modified by calcium acetate and aluminum sulfate, and the preparation method of the white silicified wood powder is as follows: the white silicified wood is crushed and ground to obtain a powder, and then the powder is added to deionized water accounting for 400% of its mass under the stirring condition of 100r / min and stirred and dispersed to obtain a powder suspension; calcium acetate solution is added to the powder suspension, the pH value is adjusted to 9.0, and then aluminum sulfate solution is added to the powder suspension under the stirring condition of 200r / min, and then reacted at 70°C and 200r / min stirring conditions for 4h, and finally cooled to room temperature, filtered, washed, and dried. The concentration of the calcium acetate solution is 1mol / L, and the amount added is 10% of the mass of the powder, and the concentration of the aluminum sulfate solution is 0.5mol / L, and the amount added is 20% of the mass of the powder.

[0098] Comparative Example 12

[0099] A whisker-reinforced UHV disc suspension porcelain insulator, the raw materials of which include: 29wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil, 6wt% quartz, and 1wt% petrified wood powder. The preparation method is the same as that of Example 3.

[0100] The silicified wood powder is a white silicified wood powder modified by calcium acetate and aluminum sulfate, and the preparation method of the white silicified wood powder is as follows: crush and grind the white silicified wood to obtain a powder, then add the powder to deionized water accounting for 450% of its mass under the stirring condition of 200r / min and stir and disperse to obtain a powder suspension; add calcium acetate solution to the powder suspension, adjust the pH value to 9.2, then add aluminum sulfate solution to the powder suspension under the stirring condition of 280r / min, then react at 80°C and 250r / min stirring conditions for 3.5h, finally cool to room temperature, filter, wash, and dry. The concentration of the calcium acetate solution is 2mol / L, and the amount added is 8% of the mass of the powder, and the concentration of the aluminum sulfate solution is 0.8mol / L, and the amount added is 15% of the mass of the powder.

[0101] Comparative Example 13

[0102] A whisker-reinforced UHV disc suspension porcelain insulator, the raw materials of which include: 28wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil, 6wt% quartz, and 2wt% petrified wood powder. The preparation method is the same as that of Example 3.

[0103] The silicified wood powder is a white silicified wood powder modified by calcium acetate and aluminum sulfate, and the preparation method of the white silicified wood powder is as follows: crush and grind the white silicified wood to obtain a powder, then add the powder to deionized water accounting for 500% of its mass under the stirring condition of 300r / min and stir and disperse to obtain a powder suspension; add calcium acetate solution to the powder suspension, adjust the pH value to 9.5, then add aluminum sulfate solution to the powder suspension under the stirring condition of 350r / min, and then react at 90°C and 300r / min stirring conditions for 3h, and finally cool to room temperature, filter, wash, and dry. The concentration of the calcium acetate solution is 3mol / L, and the amount added is 5% of the mass of the powder, and the concentration of the aluminum sulfate solution is 1.2mol / L, and the amount added is 10% of the mass of the powder.

[0104] Comparative Example 14

[0105] A whisker-reinforced UHV disc suspension porcelain insulator, the raw materials of which include: 29wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil, 6wt% quartz, and 1wt% petrified wood powder. The preparation method is the same as that of Example 3.

[0106] The petrified wood powder is white petrified wood powder, which is a powder obtained by crushing and grinding white petrified wood without any modification treatment.

[0107] Comparative Example 15

[0108] A whisker-reinforced UHV disc suspension porcelain insulator, the raw materials of which include: 29wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil, 6wt% quartz, and 1wt% petrified wood powder. The preparation method is the same as that of Example 3.

[0109] The petrified wood powder is brown petrified wood powder modified by calcium acetate and aluminum sulfate, and the preparation method of brown petrified wood powder is as follows: the brown petrified wood is crushed and ground to obtain powder, and then the powder is added to deionized water accounting for 450% of its mass under the stirring condition of 200r / min and stirred and dispersed to obtain a powder suspension; calcium acetate solution is added to the powder suspension, the pH value is adjusted to 9.2, and then aluminum sulfate solution is added to the powder suspension under the stirring condition of 280r / min, and then reacted at 80°C and 250r / min for 3.5h, and finally cooled to room temperature, filtered, washed, and dried. The concentration of calcium acetate solution is 2mol / L, and the amount added is 8% of the mass of the powder, and the concentration of aluminum sulfate solution is 0.8mol / L, and the amount added is 15% of the mass of the powder.

[0110] Comparative Example 16

[0111] A whisker-reinforced UHV disc suspension porcelain insulator, the raw materials of which include: 29wt% alumina powder, 16wt% ball clay, 15wt% feldspar, 15wt% Fujian mud, 9wt% andalusite, 9wt% ash soil, 6wt% quartz, and 1wt% petrified wood powder. The preparation method is the same as that of Example 3.

[0112] The silicified wood powder is reddish brown silicified wood powder modified by calcium acetate and aluminum sulfate, and the preparation method of the reddish brown silicified wood powder is as follows: crush and grind the reddish brown silicified wood to obtain a powder, then add the powder to deionized water accounting for 450% of its mass under the stirring condition of 200r / min and stir and disperse to obtain a powder suspension; add calcium acetate solution to the powder suspension, adjust the pH value to 9.2, then add aluminum sulfate solution to the powder suspension under the stirring condition of 280r / min, then react at 80°C and 250r / min stirring conditions for 3.5h, finally cool to room temperature, filter, wash, and dry. The concentration of the calcium acetate solution is 2mol / L, and the amount added is 8% of the mass of the powder, and the concentration of the aluminum sulfate solution is 0.8mol / L, and the amount added is 15% of the mass of the powder.

[0113] According to the same testing method as in (III) above, the performance of the porcelain insulator samples prepared in Comparative Examples 11-16 was tested, and the test results were statistically obtained in the following Table 6:

[0114] Table 6: Performance test results of comparative examples 11-16

[0115]

[0116] It can be seen from Table 6 above that adding white silicified wood powder modified by calcium acetate and aluminum sulfate to the raw materials can significantly improve the flexural strength of the sample, and the volume density and porosity data are also improved to a certain extent. Among them, when 0.2% white silicified wood powder is added, the flexural strength is increased by 4.9% compared with Example 3, and when 1% white silicified wood powder is added, the flexural strength is increased by 10.4% compared with Example 3. The increase increases with the increase in the amount of white silicified wood powder, indicating that the white silicified wood powder plays a promoting role. When 2% white silicified wood powder is added, the flexural strength is increased by 11.5% compared with Example 3. Although the increase is not much compared with the 2% dosage, it is still very significant. In addition, it can be seen from Comparative Example 14 that the addition of white silicified wood powder that has not been modified with calcium acetate and aluminum sulfate has no effect on improving the performance of the sample, and even shows a downward trend in bending strength, which shows that the modification process is very important; it can be seen from Comparative Examples 15 and 16 that the addition of brown silicified wood powder and reddish-brown silicified wood powder, even after modification, has no obvious effect on improving the performance of the sample.

[0117] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A whisker-reinforced UHV disc-shaped suspension porcelain insulator, characterized in that: The raw materials of the porcelain insulator include: 26-35wt% alumina powder, 15-20wt% ball clay, 14-19wt% feldspar, 10-15wt% Fujian mud, 6-12wt% andalusite, 6-12wt% ash soil, 6-9wt% quartz, and 0.2-2wt% petrified wood powder; The mass ratio of the andalusite to the ash soil is 1:1, the silicified wood powder is white silicified wood powder modified by calcium acetate and aluminum sulfate, and the preparation method of the white silicified wood powder is as follows: the white silicified wood is crushed and ground to obtain a powder, and then the powder is added to deionized water accounting for 400% to 500% of the mass of the powder under the stirring condition of 100 to 300 r / min and stirred and dispersed to obtain a powder suspension; calcium acetate solution is added to the powder suspension, the pH value is adjusted to 9.0 to 9.5, and then aluminum sulfate solution is added to the powder suspension under the stirring condition of 200 to 350 r / min, and then the reaction is carried out at a temperature of 70 to 90° C. and a stirring condition of 200 to 300 r / min for 3-4 hours, and finally cooled to room temperature, filtered, washed, and dried; The concentration of the calcium acetate solution is 1-3 mol / L, and the amount added is 5-10% of the mass of the powder. The concentration of the aluminum sulfate solution is 0.5-1.2 mol / L, and the amount added is 10-20% of the mass of the powder.

2. A whisker-reinforced UHV disc-shaped suspension porcelain insulator according to claim 1, characterized in that: The Al2O3 content in the andalusite and ash soil is greater than 55wt%.

3. A method for preparing a whisker-reinforced UHV disc-shaped suspension porcelain insulator as claimed in any one of claims 1 to 2, characterized in that the steps include: S1. Alumina powder, ball clay, feldspar, Fujian mud, andalusite, ash soil, quartz, and white silicified wood powder are mixed in proportion and then wet-milled to obtain a mixed abrasive; S2, screening the mixed abrasive to remove iron, and then squeezing mud to obtain mud cake and aging it; S3, extruding the mud cake in a vacuum mud kneading machine to obtain a blank; S4, using an aluminum mold cloth lining pressure to make a blank, wet spinning the blank into shape, and drying to obtain a green blank; S5. After glazing, sanding, firing and inspecting the green body, the whisker-reinforced UHV disc-shaped suspension porcelain insulator with in-situ generated mullite is obtained.

4. The method for preparing the whisker-reinforced UHV disc-shaped suspension porcelain insulator according to claim 3, characterized in that: In step S1, during wet ball milling, the mass ratio of the blank particles, water and balls is 1:1:2, and the ball milling time is 30-35 hours; In step S2, the high-strength slurry is screened for 3 times for iron removal, the high-strength slurry is iron removed for 3 times, the slurry fineness during the mud squeezing process is 0.1% to 0.2% of the 325-mesh sieve residue, the aging time is 80-100h, the aging chamber temperature is 15-30°C, and the aging chamber humidity is 75%; In step S3, the moisture difference of the mud sections put into the mud making machine during extrusion is ≤0.5%, and the relative vacuum degree of the vacuum mud making machine is ≥96%; In step S4, the moisture content of the wet spinning blank is 17.3% to 17.8%, the drying temperature is 40 to 60° C., and the drying time is 100 to 130 hours; In step S5, the gas supply pressure of the burning gas is 6-7KPa, the gas working pressure is ≥1.5KPa, the burning temperature is 1280±10℃, and the burning time is 75m 3 Gas drawer kiln 48h, or 180m 3 Gas drawer kiln 39h.