A floor material with Class A fireproof functionality and production method thereof
By using the flame retardant functional components prepared by sodium alginate and aramid fibers loading with accumulationite in epoxy resin floor materials, a triad integrated expansion flame retardant system and a miniature three-dimensional structure are formed, and the epoxy resin-like land is solved. The problems of poor fire resistance and poor wear resistance of the flat materials have achieved excellent Class A fire resistance and wear resistance, extending the service life.
Patent Information
- Application Number
- CN202410475424.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-19
AI Technical Summary
Epoxy resin floor materials have poor fire resistance and poor wear resistance, making it difficult to meet the dual needs of modern buildings for fire resistance and wear resistance.
Sodium alginate is used as raw material to prepare flame retardant functional components, combined with aramid fiber loaded with accumulation stone as modified fiber components, the three-in-one expansion flame retardant system and micro three-dimensional structure are formed in epoxy resin to enhance the ground Fire resistance and wear resistance of flat materials.
It significantly improves the A-level fire-retardant and wear-resistant properties of epoxy resin floor materials, extends the service life, and enhances the hardness and stress dispersing ability of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of material technology, and in particular to a floor material with Class A fireproof functionality and a production method thereof. Background Art
[0002] In recent years, with the rapid development of the construction industry, the demand for floor materials has been increasing. So far, floor materials have been relatively mature and are currently divided into three types, namely epoxy resin, acrylic and polyurethane. Among them, epoxy resin floor materials have good pressure resistance and corrosion resistance, and can be widely used in various places, making the floor surface smoother and easier to clean and maintain. Due to the frequent occurrence of fire accidents in recent years, the fireproof performance of building materials has gradually attracted people's attention. Epoxy resin itself is a polymer material, which is easy to burn and difficult to meet the demand for fireproof floor materials. In addition, since floor materials need to rub against objects for a long time, they also need to maintain good wear resistance. Therefore, floor materials based on epoxy resin need to enhance wear resistance in order to be better applied.
[0003] In order to solve the related problems of epoxy resin floor materials, the current main method is to use additives. For example, the invention patent with publication number CN111925719A discloses a fire-retardant floor coating and a preparation method thereof. By adding boric acid compounds and metal hydroxides as additives, metal oxides and the like are generated on the surface of the coating during the combustion process to protect the coating, thereby improving the fire retardant properties of the coating. However, this technical solution does not pay attention to the wear resistance of the epoxy resin floor material. It only relies on the wear resistance of the epoxy resin itself and cannot cope with long-term friction environments such as factories and parking lots.
[0004] Based on this, the present invention provides an epoxy resin floor material, which has excellent fire resistance and wear resistance, can further broaden the application of epoxy resin floor coatings, and has a longer service life. Summary of the invention
[0005] The purpose of the present invention is to provide a floor material with Class A fireproof functionality and a production method thereof, which solves the problem that the epoxy resin floor material has poor fireproof performance and poor wear resistance.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A floor material with Class A fireproof functionality, comprising an A component and a B component;
[0008] The A component includes the following raw materials in parts by weight:
[0009] Epoxy resin 30-45 parts;
[0010] 3-5 parts of flame retardant functional components;
[0011] 4-8 parts of modified fiber component;
[0012] Defoaming agent 0.1-0.3 parts;
[0013] Leveling agent 0.1-0.3 parts;
[0014] 2-5 parts of diluent;
[0015] Wetting agent 0.3-0.6 parts;
[0016] 5-15 parts of inorganic filler;
[0017] The B component includes the following raw materials in parts by weight:
[0018] 15-25 parts of amine curing agent;
[0019] The production method comprises the following steps:
[0020] The first step is to add the raw materials in component A into a mixer, and stir and mix at a rate of 300-400 r / min for 10-20 min to form a mixture;
[0021] Step 2: Add the raw materials of component B into the mixture. After adding, adjust the speed to 800-1000r / min, stir and mix for 20-30min, let it stand for 10-20min, and then discharge the material.
[0022] As a further embodiment of the present invention, the defoaming agent is polyether modified polysiloxane; the leveling agent is BYK-310 or BYK-315N; the diluent is a glycidyl ether active diluent; the wetting agent is polyoxyethylene alkylphenol ether; and the inorganic filler is at least one of talc, fumed silica, titanium dioxide or calcium carbonate.
[0023] A floor material with Class A fireproof functionality is produced using the above production method.
[0024] As a further solution of the present invention, the specific preparation method of the flame retardant functional component is as follows:
[0025] Step 1: Make biomass intermediate material
[0026] Sodium alginate and dimethyl sulfoxide are mixed and stirred evenly, and then halogen-substituted isocyanate and alkaline catalyst are added to the mixed solution. After the addition is completed, heating is turned on and the temperature is maintained at 50-60°C. After mechanical stirring for 2-4 hours, the temperature is lowered and the material is discharged to obtain a biomass intermediate material;
[0027] Step 2: Make flame retardant functional components
[0028] Add the biomass intermediate material and the phosphate derivative containing substituted hydroxyl groups into N,N-dimethylformamide, stir until a uniform mixed liquid is formed, increase the temperature to 70-80°C, add a metal tin catalyst, stir for 2-4 hours, and then discharge the material to obtain a flame retardant functional component.
[0029] Specifically, in step one, the sodium alginate structure contains substituted hydroxyl groups, which can be substituted with the halogen functional groups in the halogen-substituted isocyanate structure under the action of an alkaline catalyst to obtain a sodium alginate biomass intermediate material containing an isocyanate active group in the structure. In step two, the isocyanate active group further reacts with the phosphate derivative containing the substituted hydroxyl group under the action of a metal tin catalyst, thereby further introducing a phosphorus flame retardant into the sodium alginate structure, and finally obtaining a flame retardant functional component.
[0030] Among the flame-retardant functional components, sodium alginate can be used as a carbon source, and its structure also contains nitrogen and phosphorus sources produced by chemical modification, which can form a ternary intumescent flame retardant system. This allows a smaller amount of addition to effectively improve the flame retardant properties of epoxy resin floor materials.
[0031] As a further embodiment of the present invention, in step 1, the alkaline catalyst is triethylamine or pyridine.
[0032] As a further embodiment of the present invention, in step 1, the halogen-substituted isocyanate is 2-chloroethyl isocyanate or 3-chloropropyl isocyanate.
[0033] As a further embodiment of the present invention, in step 2, the metal tin catalyst is at least one of stannous octoate, dibutyltin dilaurate or dibutyltin diacetate.
[0034] As a further embodiment of the present invention, in step 2, the 2-hydroxyethyl dimethyl phosphate or pentaerythritol phosphate.
[0035] As a further embodiment of the present invention, the specific preparation method of the modified fiber component is as follows:
[0036] Step S1: Making modified rectorite
[0037] The rectorite and aniline monomer are put into a hydrochloric acid solution, and ultrasonically dispersed to form a uniform dispersion. The dispersion is placed in an ice bath, and ammonium persulfate is added to the dispersion at a stirring rate of 3000-4000 r / min. After the addition is completed, the stirring is continued for 12-24 hours, and the solid material is separated to obtain the modified rectorite;
[0038] Step S2: preparing modified fiber components
[0039] The modified rectorite and aramid fiber are mixed with toluene, ultrasonically dispersed at an ultrasonic frequency of 60-80kHz for 30-40 minutes, and then the temperature is increased to 80-90°C. After stirring at a rate of 1000-2000r / min for 4-6 hours, the material is cooled and discharged. The material is placed in a ball mill and the ball milling treatment is continued for 2-4 hours to obtain the modified fiber component.
[0040] Specifically, in step S1, ammonium persulfate is used as an initiator to initiate in-situ polymerization of aniline on the surface of rectorite to form a modified rectorite coated with polyaniline. In step S2, since the polyaniline structure contains a benzene ring aromatic structure, it can form an aromatic π-π conjugated system with the aromatic benzene ring in the aramid fiber under high temperature and ball milling conditions, thereby tightly combining the rectorite with the aramid fiber to form an aramid fiber loaded with rectorite, that is, a modified fiber component.
[0041] As a further solution of the present invention, in step S1, the concentration of the hydrochloric acid solution is 1-2 mol / L.
[0042] As a further solution of the present invention, in step S2, the mass ratio of the modified rectorite to the aramid fiber is 1:3-5.
[0043] Beneficial effects of the present invention:
[0044] 1) The present invention uses sodium alginate as a raw material to prepare a flame retardant functional component, and utilizes its ternary special expansion flame retardant system to quickly form an expansion carbon layer when the floor material burns, which can greatly improve the fire retardant performance of the epoxy resin floor coating, and this purpose can be achieved without a large amount of addition.
[0045] 2) The present invention uses aramid fiber loaded with rectorite as a modified fiber component. After adding it to epoxy resin, the "ball" effect formed by rectorite and aramid fiber can be used to improve the wear resistance of the floor material. In addition, after the aramid fiber is loaded with rectorite, it can form a miniature three-dimensional structure. Since the polyaniline structure coated on the surface of the rectorite contains an amino active structure, it can participate in the curing process of the epoxy resin floor material, thereby producing a skeleton support effect in the floor material, thereby playing a good role in dispersing stress and transferring loads, and enhancing the hardness and other properties of the floor material. Moreover, rectorite can form a high-temperature resistant barrier during the combustion process, and can cooperate with the flame retardant functional component to further enhance the fire retardant properties of the floor material.
[0046] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. DETAILED DESCRIPTION
[0047] The technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] Example 1
[0049] A floor material with Class A fireproof functionality, comprising an A component and a B component;
[0050] The A component includes the following raw materials in parts by weight:
[0051] 128 Epoxy resin 30 parts;
[0052] 3 parts of flame retardant functional components;
[0053] 4 parts of modified fiber component;
[0054] 0.1 part of polyether modified polysiloxane;
[0055] BYK-310 0.1 part;
[0056] 2 parts of ethylene glycol diglycidyl ether;
[0057] 0.3 parts of polyoxyethylene alkylphenol ether;
[0058] 5 parts of talcum powder;
[0059] The B component includes the following raw materials in parts by weight:
[0060] 15 parts of polyetheramine;
[0061] The production method of the floor material comprises the following steps:
[0062] The first step is to add the raw materials in component A into a mixer and stir and mix at a rate of 300 r / min for 20 min to form a mixture;
[0063] Step 2: Add the raw materials of component B into the mixture. After adding, adjust the speed to 800r / min, stir and mix for 30 minutes, let it stand for 10 minutes, and then discharge the material.
[0064] Example 2
[0065] A floor material with Class A fireproof functionality, comprising an A component and a B component;
[0066] The A component includes the following raw materials in parts by weight:
[0067] 128 epoxy resin 40 parts;
[0068] 4.5 parts of flame retardant functional components;
[0069] 5 parts of modified fiber component;
[0070] 0.2 parts of polyether modified polysiloxane;
[0071] BYK-315N 0.2 parts;
[0072] 4 parts of ethylene glycol diglycidyl ether;
[0073] 0.4 parts of polyoxyethylene alkylphenol ether;
[0074] 6 parts of fumed silica;
[0075] The B component includes the following raw materials in parts by weight:
[0076] 20 parts of polyetheramine;
[0077] The production method of the floor material comprises the following steps:
[0078] The first step is to add the raw materials in component A into a mixer, and stir and mix at a rate of 400 r / min for 10 minutes to form a mixture;
[0079] Step 2: Add the raw materials of component B into the mixture. After adding, adjust the speed to 1000r / min, stir and mix for 20 minutes, let it stand for 20 minutes, and then discharge the material.
[0080] Example 3
[0081] A floor material with Class A fireproof functionality, comprising an A component and a B component;
[0082] The A component includes the following raw materials in parts by weight:
[0083] 128 epoxy resin 45 parts;
[0084] 5 parts of flame retardant functional components;
[0085] 8 parts of modified fiber component;
[0086] 0.3 parts of polyether modified polysiloxane;
[0087] BYK-315N 0.3 parts;
[0088] 5 parts of ethylene glycol diglycidyl ether;
[0089] 0.6 parts of polyoxyethylene alkylphenol ether;
[0090] 15 parts of calcium carbonate;
[0091] The B component includes the following raw materials in parts by weight:
[0092] 25 parts of polyetheramine;
[0093] The production method of the floor material comprises the following steps:
[0094] The first step is to add the raw materials in component A into a mixer, and stir and mix at a rate of 400 r / min for 20 minutes to form a mixture;
[0095] Step 2: Add the raw materials of component B into the mixture. After adding, adjust the speed to 1000r / min, stir and mix for 20 minutes, let it stand for 20 minutes, and then discharge the material.
[0096] Comparative Example 1
[0097] A floor material, which is different from Example 2 in that no flame retardant functional component is added, and the rest is the same as Example 2.
[0098] Comparative Example 2
[0099] A floor material, which is different from Example 2 in that no modified fiber component is added, and the rest is the same as Example 2.
[0100] Comparative Example 3
[0101] A floor material, which is different from Example 2 in that the modified fiber component is replaced with aramid fiber, and the rest is the same as Example 2.
[0102] The flame retardant functional components in the above examples and comparative examples were prepared by the following method:
[0103] Step 1: Make biomass intermediate material
[0104] 3.2 g of sodium alginate and dimethyl sulfoxide were mixed and stirred evenly, and then 1.5 g of 2-chloroethyl isocyanate and 1.2 g of triethylamine were added to the mixture. After the addition was completed, heating was turned on and the temperature was maintained at 55°C. After mechanical stirring for 3 hours, the temperature was lowered and the material was discharged to obtain a biomass intermediate material;
[0105] The percentage of isocyanate groups in the biomass intermediate was tested using the acetone-di-n-butylamine titration method, and the result was 9.82%;
[0106] Step 2: Make flame retardant functional components
[0107] Add 2.6 g of biomass intermediate material and 1.2 g of pentaerythritol phosphate to N,N-dimethylformamide, stir until a uniform mixture is formed, increase the temperature to 75°C, add 0.2 g of dibutyltin dilaurate, stir for 3 hours, and then discharge the material to obtain a flame retardant functional component.
[0108] The acetone-di-n-butylamine titration method was also used to test the percentage of isocyanate groups in the flame retardant functional component, and the result was 1.09%. This was due to the amine esterification reaction between the isocyanate groups and the hydroxyl groups of pentaerythritol phosphate, resulting in a large consumption of isocyanate groups.
[0109] The modified fiber components in the above examples and comparative examples were prepared by the following method:
[0110] Step S1: Making modified rectorite
[0111] 8 g of rectorite and 6.5 g of aniline monomer were put into 100 mL of 1 mol / L hydrochloric acid solution, and ultrasonically dispersed to form a uniform dispersion. The dispersion was placed in an ice bath, and 0.2 g of ammonium persulfate was added to the dispersion at a stirring rate of 3500 r / min. After the addition was completed, stirring was continued for 18 h, and the solid material was separated to obtain modified rectorite;
[0112] Accurately weigh 0.5 g of modified rectorite, and use XKCHN-700 element analyzer to analyze its organic element content. The test results show that the percentage of carbon element is 34.05%, and the percentage of nitrogen element is 5.87%. Since rectorite does not contain these organic elements, these organic elements are derived from the polyaniline coated on the surface of rectorite;
[0113] Step S2: preparing modified fiber components
[0114] 4.5 g of modified rectorite and 15 g of aramid fiber were mixed with toluene, and ultrasonically dispersed at an ultrasonic frequency of 80 kHz for 30 min. The temperature was then raised to 90°C, and stirred at a rate of 1500 r / min for 6 h. The material was cooled and discharged, and the material was placed in a ball mill and continued to be ball-milled for 3 h to obtain the modified fiber component.
[0115] Test Case
[0116] The floor materials in Examples 1 to 3 and Comparative Examples 1 to 3 were made into coating films, and the following performance tests were performed:
[0117] Fire rating test is carried out according to GB 8624-2012 "Classification of Combustion Performance of Building Materials and Products";
[0118] According to GB / T 1768-2006 "Determination of abrasion resistance of paints and varnishes - Rotating rubber grinding wheel method", the abrasion resistance test was carried out under the test conditions of 750g and 500r;
[0119] According to GB / T 6739-2006 “Determination of film hardness by pencil method for paints and varnishes”, test the hardness of the sample;
[0120] The results are shown in Table 1:
[0121] Table 1 - Test results
[0122] From the test results in Table 1, it can be seen that the fire resistance grade of the floor material with flame retardant functional components and fiber modified components as additives reaches Class A, with excellent fire retardant properties, and also excellent wear resistance and hardness.
[0123] After removing the flame retardant functional components, the fire resistance level of the floor material is significantly reduced.
[0124] After removing the wear-resistant modified components, the wear resistance and pencil hardness of the floor material decreased significantly, and the fire resistance level was affected to a certain extent. This proves that the presence of rectorite can cooperate with the flame retardant functional components to improve the fire retardant properties of the floor material.
[0125] After replacing the wear-resistant modified component with aramid fiber, the wear resistance and hardness of the floor material are improved, indicating that the addition of aramid fiber can have a reinforcing effect on the floor material to a certain extent.
[0126] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
[0127] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for producing a floor material with Class A fireproof functionality, characterized in that: The floor material comprises component A and component B; The A component includes the following raw materials in parts by weight: Epoxy resin 30-45 parts; 3-5 parts of flame retardant functional components; 4-8 parts of modified fiber component; Defoaming agent 0.1-0.3 parts; Leveling agent 0.1-0.3 parts; 2-5 parts of diluent; Wetting agent 0.3-0.6 parts; 5-15 parts of inorganic filler; The B component includes the following raw materials in parts by weight: 15-25 parts of amine curing agent; The production method comprises the following steps: The first step is to add the raw materials in component A into a mixer, and stir and mix at a rate of 300-400 r / min for 10-20 min to form a mixture; Step 2: Add the raw materials of component B to the mixture. After adding, adjust the speed to 800-1000r / min, stir and mix for 20-30min, let it stand for 10-20min, and then discharge the mixture. The specific preparation method of the flame retardant functional component is as follows: Step 1: Make biomass intermediate material Sodium alginate and dimethyl sulfoxide are mixed and stirred evenly, and then halogen-substituted isocyanate and alkaline catalyst are added to the mixed solution. After the addition is completed, heating is turned on and the temperature is maintained at 50-60°C. After mechanical stirring for 2-4 hours, the temperature is lowered and the material is discharged to obtain a biomass intermediate material; Step 2: Make flame retardant functional components Add the biomass intermediate material and the phosphate derivative containing substituted hydroxyl groups to N,N-dimethylformamide, stir until a uniform mixed solution is formed, increase the temperature to 70-80°C, add a metal tin catalyst, stir for 2-4 hours, and then discharge the material to obtain a flame retardant functional component; The specific preparation method of the modified fiber component is as follows: Step S1: Making modified rectorite The rectorite and aniline monomer are put into a hydrochloric acid solution, and ultrasonically dispersed to form a uniform dispersion. The dispersion is placed in an ice bath, and ammonium persulfate is added to the dispersion at a stirring rate of 3000-4000 r / min. After the addition is completed, the stirring is continued for 12-24 hours, and the solid material is separated to obtain the modified rectorite; Step S2: preparing modified fiber components The modified rectorite and aramid fiber are mixed with toluene, ultrasonically dispersed at an ultrasonic frequency of 60-80kHz for 30-40 minutes, and then the temperature is increased to 80-90°C. After stirring at a rate of 1000-2000r / min for 4-6 hours, the material is cooled and discharged. The material is placed in a ball mill and the ball milling treatment is continued for 2-4 hours to obtain the modified fiber component.
2. The method for producing a floor material with Class A fireproof functionality according to claim 1, characterized in that: In step 1, the alkaline catalyst is triethylamine or pyridine.
3. The method for producing a floor material with Class A fireproof functionality according to claim 1, characterized in that: In step 1, the halogen-substituted isocyanate is 2-chloroethyl isocyanate or 3-chloropropyl isocyanate.
4. The method for producing a floor material with Class A fireproof functionality according to claim 1, characterized in that: In step 2, the metal tin catalyst is at least one of stannous octoate, dibutyltin dilaurate or dibutyltin diacetate.
5. The method for producing a floor material with Class A fireproof functionality according to claim 1, characterized in that: In step 2, the phosphate derivative containing a substituted hydroxyl group is 2-hydroxyethyl dimethyl phosphate or pentaerythritol phosphate.
6. The method for producing a floor material with Class A fireproof functionality according to claim 1, characterized in that: In step S1, the concentration of the hydrochloric acid solution is 1-2 mol / L.
7. The method for producing a floor material with Class A fireproof functionality according to claim 1, characterized in that: In step S2, the mass ratio of the modified rectorite to the aramid fiber is 1:3-5.
8. A floor material with Class A fireproof functionality, characterized in that: The method is prepared by the production method as claimed in claim 1.
Citation Information
Patent Citations
Fireproof floor coating and preparation method thereof
CN111925719A
High-performance water-based anticorrosion paint and preparation method thereof
CN102134410A
Ship heavy-duty anti-corrosive coating with double anti-corrosive functions and preparation method thereof
CN102634265A
Single-component waterproof flame-retardant polyurethane coating
CN108456483A
Self-flame-retardant oleth-2 phosphate terminated polyurethane waterborne coating
CN110951304A