A laser cladding online metallurgical process

By adding powders with missing alloy components to the surface of the substrate in the laser cladding process and using laser cladding technology and combined with arc welding, the problem of missing alloy components of the wire is solved, and efficient and economical coating components are achieved. Improved cladding effect.

CN118291972BActive Publication Date: 2024-12-06SHANGHAI GZCLAD LASER TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410569658.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-12-06
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

In laser cladding process, wire materials are widely used due to their low cost, but they may lack some alloy components, which makes the surface coating components of the substrate unable to meet the requirements, and the prior art is difficult to effectively solve this problem.

Method used

Using laser cladding online metallurgy process, by cleaning the surface of the substrate and adding powder materials with missing alloy components to it, using a laser beam to cladd the wire and powder materials on the surface of the substrate to form a coating, and perform surface treatment. Combined with arc welding technology to improve cladding effect.

Benefits of technology

On the premise of reducing costs, the requirements for coating composition on the substrate surface are met, the cladding effect and cost-effectiveness are improved, and the performance and quality of the coating are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118291972B_ABST
    Figure CN118291972B_ABST
Patent Text Reader

Abstract

The present application discloses an online metallurgical process for laser cladding, which relates to the field of laser cladding, and includes the following steps: S1: cleaning the required cladding area on the surface of the substrate; S2: adding wire to the surface of the substrate, and adding powder to the surface of the substrate at the same time, the powder is the alloy component missing in the wire, and using a first laser beam to clad the wire and powder on the surface of the substrate; S3: forming a coating, and combining it with the surface of the substrate after cooling; S4: surface treating the coating. The present application solves the problem of meeting the requirements of the substrate surface for the coating component when the wire lacks some alloy components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of laser cladding, and in particular to an online metallurgical process for laser cladding. Background Art

[0002] The main purpose of laser cladding is to deposit a metal coating on the surface of a metal substrate to improve its surface properties, such as hardness, wear resistance, corrosion resistance, etc. The birth of this technology provides a new method for the surface treatment of metal materials, which significantly improves the service life of metal materials.

[0003] In the laser cladding process, the required metal raw material powders need to be mixed together, and the powders are sprayed onto the surface of the substrate during cladding. The laser is used as a heat source to form a molten pool between the powder and the substrate surface, which is then cooled to form a coating on the substrate surface to improve the performance of the substrate.

[0004] In the actual production process, wire is often used instead of powder for cladding operations due to its low cost. However, since wire is drawn, it may not contain all the required components. If the wire forming formula needs to be modified to form the wire with the required components, the cost is relatively high. Therefore, it is urgent to invent an online metallurgical process for laser cladding to solve the problem of meeting the coating composition requirements on the substrate surface when the wire lacks some alloy components. Summary of the invention

[0005] In order to solve the problem of a wire lacking some alloy components and satisfying the requirements of the substrate surface for the coating composition, the present application provides a laser cladding online metallurgical process.

[0006] The laser cladding online metallurgical process provided in this application adopts the following technical solution:

[0007] A laser cladding online metallurgical process comprises the following steps:

[0008] S1: Clean the required cladding area on the substrate surface;

[0009] S2: adding wire to the surface of the substrate, and adding powder to the surface of the substrate at the same time, the powder is the alloy component missing in the wire, and using the first laser beam to clad the wire and the powder on the surface of the substrate;

[0010] S3: forming a coating, which combines with the substrate surface after cooling;

[0011] S4: Perform surface treatment on the coating.

[0012] By adopting the above technical solution, the surface of the substrate is first cleaned, such as degreasing and grinding, to ensure the cleanliness of the substrate surface, and then the wire is added to the substrate surface by a wire feeder. Since the wire lacks some alloy components, powder is used to supplement it, that is, powder is added to the substrate surface at the same time. During the adding process, the first laser beam is used to melt the wire and powder on the substrate surface, and finally a coating is formed on the substrate surface. After cooling, polishing and other surface treatments are performed. In this way, the requirements of the substrate surface for the coating composition are met under the premise of saving costs by using wire.

[0013] Preferably, in step S2, powder is fed coaxially within the first laser beam and wire is fed outside the first laser beam.

[0014] By adopting the above technical solution, a light beam is used, powder is coaxially fed inside the light, and wire is fed outside the light, so that cladding of powder material and wire material is achieved at the convergence point of the first laser beam.

[0015] Preferably, in step S2, arc welding is used to melt and weld the additive material during wire feeding.

[0016] By adopting the above technical solution, arc welding and laser heating are used for welding, which makes up for the shortcomings of laser energy loss and low electro-optical conversion efficiency, that is, high energy density, high energy utilization rate and high arc stability are achieved.

[0017] Preferably, in step S2, the wire is coaxially fed within the first laser beam, and the powder is fed outside the first laser beam.

[0018] By adopting the above technical solution, a light beam is used, the wire is coaxially fed inside the light, and the powder is fed outside the light, so that the cladding of the powder material and the wire material is achieved at the convergence point of the first laser beam.

[0019] Preferably, in step S2, powder is fed inside or outside the first laser beam, and a second laser beam is used to feed wire inside or outside the second laser beam.

[0020] By adopting the above technical solution, two light beams are used, one light beam is used to clad the powder material, and the other light beam is used to clad the wire material, thereby increasing the energy and helping to achieve a better cladding effect.

[0021] Preferably, in step S2, if there are two wires, the two wires can be twisted to form a pair of twisted wires, and if there are multiple wires, multiple twisted wires can be formed, and then the wires are transported.

[0022] By adopting the above technical solution, when there are two missing wires, two wires are needed during cladding. The two wires are twisted together in advance to form a pair of twisted wires, that is, after subsequent melting, the two are highly mixed, which helps to improve the cladding effect; similarly, when multiple wires are needed, they are twisted into multiple twisted wires, which also has a better cladding effect.

[0023] Preferably, the powder feeder comprises a shell, a plurality of powder feeding pipes are connected to the upper side of the shell, a powder feeding port is formed on the lower side of the shell, and a quantitative mixing structure is arranged in the shell, which can quantitatively mix the various powders introduced into the shell.

[0024] By adopting the above technical solution, when the powder is pumped into the shell, quantitative mixing of the powder can be achieved through the quantitative mixing mechanism. On the one hand, the amount of powder can be controlled, and on the other hand, the mixing uniformity of the two can be improved, which helps to improve the cladding effect.

[0025] Preferably, the quantitative mixing mechanism includes a material receiving tray, a quantitative tray and a leakage tray, the material receiving tray is arranged in the shell and has a plurality of material receiving holes, the quantitative tray is rotatably connected to the shell and is located below the material receiving tray, the quantitative tray has a plurality of material receiving holes, the leakage tray is arranged in the shell and is located below the quantitative tray, and has a plurality of material leakage holes; when the quantitative tray rotates until the material receiving holes are connected with the material receiving holes, all the material receiving holes and all the leakage holes are staggered, and when the quantitative tray rotates until the material receiving holes are connected with the leakage holes, the powder leaks out from the leakage holes.

[0026] By adopting the above technical scheme, when the powder is drawn from the powder feeding pipe into the receiving plate, the powder enters the receiving hole and then enters the containing hole. At this time, the containing hole is not connected with the leakage hole. Then the quantitative plate rotates, and the containing hole filled with powder is connected with the leakage hole. The powder can fall down and be discharged from the powder feeding port. The quantitative feeding of the powder can be achieved by the quantitative plate receiving the powder and the rotation of the quantitative plate.

[0027] Preferably, the number of the material receiving holes is the same as the number of the material leakage holes, and the number of the material holding holes is twice the number of the material leakage holes.

[0028] By adopting the above technical scheme, the number of material receiving holes is the same as the number of material leakage holes, and the number of material holding holes is twice the number of material leakage holes, that is, when the material holding holes and the material receiving holes are connected, half of the material holding holes will not be connected with the material receiving holes, and at this time, these material holding holes are connected with the material leakage holes; when the material holding holes are full of powder, the quantitative disk rotates, and at this time, the material holding holes full of powder are connected with the material leakage holes, and the remaining general material holding holes are connected with the material receiving holes, and the powder material continues to be received, that is, the material is received while the material is leaking, which helps to improve the efficiency of the leakage.

[0029] Preferably, the quantitative mixing mechanism also includes a rubber spring arranged in the shell, the rubber spring is located below the leakage tray, the rubber spring is in a truncated cone shape, and the smaller end of the rubber spring is located on the side away from the leakage tray, and the shell is located below the rubber spring and is funnel-shaped.

[0030] By adopting the above technical solution, when powder leaks out from the leakage plate, the powder will fall on the rubber dome. Since there is a certain height difference between the leakage plate and the rubber dome, the powder will bounce and rebound when it falls on the rubber dome under the action of gravity. Different powders are mixed together during the bouncing process. Since the powder is dispersed more during the bouncing process, the mixing uniformity will be higher. Then the powder will leak out from the lower port of the rubber dome and finally be discharged from the powder feeding port.

[0031] Preferably, a driving motor is provided on the shell, and the output shaft of the driving motor passes through the shell and is connected to the quantitative disk. The driving motor drives the quantitative disk to rotate intermittently. A driving rod is provided on the lower side of the quantitative disk, and a connecting rod is provided on the larger port of the connecting rubber spring sheet, and the driving rod and the connecting rod are connected.

[0032] By adopting the above technical solution, the driving motor is operated, and the driving motor drives the metering disk to rotate intermittently to realize intermittent feeding. When the metering disk rotates intermittently, the rubber spring can be driven to rotate intermittently. When the powder falls on the rubber spring, part of the powder will adhere to the rubber spring. Compared with the intermittent rotation of the spring, the powder can slide downward, thereby improving the powder feeding effect.

[0033] Preferably, the receiving plate is provided with partitions between adjacent receiving holes, and the receiving plate is formed with arc surfaces on the peripheral sides of any receiving hole, so that the powder materials gather at the receiving holes.

[0034] By adopting the above technical solution, the material receiving holes are separated by partitions, and different material receiving holes correspond to different powder feeding pipes. The powder can easily slide into the material receiving holes through the arc surface, which is convenient for material discharge.

[0035] In summary, the present application includes at least one of the following beneficial technical effects:

[0036] 1. In order to reduce costs, when using wire, the missing alloy components are replaced by powder materials, that is, wire and powder are fed at the same time, and the base material is clad by a composite method of laser and arc welding, which has a better effect;

[0037] 2. The first laser beam and the second laser beam are used to feed powder inside or outside the first laser beam and wire inside or outside the second laser beam, which increases the energy of the laser beam acting on the powder and wire, helps to quickly clad the wire and powder, and achieves better cladding effect;

[0038] 3. When the powder is drawn into the powder feeder, the quantitative feeding of the powder is realized under the rotation of the quantitative disk. When the powder falls on the rubber dome, the powder will bounce on the rubber dome. Since the rubber dome is in a truncated cone shape, the powder will rebound to the middle axis of the rubber dome and mix the powder during the rebound process. During the rebound process, the powder will be scattered. When different powders rebound to the highest point, the powders are evenly mixed and then discharged from the lower side of the rubber dome, thus realizing the even mixing and conveying of the powders. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a process flow chart of the first embodiment of the present application;

[0040] Figure 2 This is a schematic diagram of coaxial powder feeding in the first laser beam and wire feeding outside the first laser beam in the first embodiment of the present application;

[0041] Figure 3 This is a schematic diagram of the first laser beam feeding wire inside and feeding powder outside in the second embodiment of the present application;

[0042] Figure 4 This is a schematic diagram of coaxial powder feeding in the first laser beam and coaxial wire feeding in the second laser beam in the third embodiment of the present application;

[0043] Figure 5 This is a schematic diagram of the overall structure of the powder feeder in the fourth embodiment of the present application.

[0044] Figure 6 This is an exploded view of some structures in the fourth embodiment of the present application;

[0045] Figure 7 The fourth embodiment of the present application mainly shows a schematic diagram of powder rebounding.

[0046] Figure numerals: 1. Shell; 11. Powder feeding port; 2. Powder feeding pipe; 3. Quantitative mixing mechanism; 31. Material receiving tray; 311. Material receiving hole; 32. Quantitative tray; 321. Material receiving hole; 33. Leakage tray; 331. Leakage hole; 34. Rubber spring; 4. Partition; 41. Material receiving area; 5. Driving motor; 6. Driving rod; 7. Connecting rod. DETAILED DESCRIPTION

[0047] The following is combined with Figure 1-7 This application is described in further detail.

[0048] The embodiment of the present application discloses a laser cladding online metallurgical process.

[0049] First embodiment:

[0050] Reference Figure 1 , the laser cladding online metallurgical process includes the following steps:

[0051] S1: Clean the required cladding area on the substrate surface; remove the oil stains on the substrate surface and polish the surface to ensure that the substrate surface is smooth.

[0052] S2: A wire is added to the surface of the substrate using a wire feeder, and a powder is added to the surface of the substrate using a powder feeder. The powder is the alloy component missing from the wire, and the wire and powder are clad on the surface of the substrate using a first laser beam.

[0053] S3: A coating is formed and combined with the substrate surface after cooling.

[0054] S4: Perform surface treatment on the coating, such as polishing, heat treatment, etc.

[0055] When performing cladding work, the surface of the substrate is first cleaned, the laser cladding head emits the first laser beam, the wire is fed by the wire feeder, and the powder is fed by the powder feeder. Under the action of the first laser beam, a coating is formed on the surface of the substrate. After cooling, the coating is surface treated to complete the cladding work. In practice, due to the low cost of wire materials, it is more suitable for medium and large component additive engineering applications. However, some alloy components are missing in the wire materials, which are supplemented by powder materials. Wire and powder feeding are performed at the same time to meet the requirements of the substrate surface for coating components.

[0056] In step S2, while emitting laser, arc welding is performed by using a welding machine to heat the wire and powder. Combined with laser heating, it can make up for the shortcomings of laser energy loss and low electro-optical conversion efficiency, and help to increase welding penetration and achieve efficient and high-quality welding.

[0057] Reference Figure 2 In step S2, powder is fed into the first laser beam, and wire is fed outside the first laser beam, wherein the first laser beam passes through a beam splitter to split into multiple beams, which are then converged on the surface of the substrate by a reflector. In this way, a space can be formed between the first laser beams, which is convenient for powder feeding.

[0058] In step 2, if two kinds of powders are missing, two kinds of wires are needed to be used and the two kinds of wires are wound to form a pair of twisted wires. If multiple kinds of powders are missing, multiple kinds of wires are used to be wound to form multiple twisted wires. In this way, after heating, the materials are mixed more evenly and the degree of mixing is high, which helps to improve the cladding effect.

[0059] Second embodiment: Reference Figure 3 , wire is fed in the first laser beam and powder is fed outside the second laser beam.

[0060] The third embodiment: Figure 4, powder is fed inside or outside the first laser beam, and a second laser beam is also used to feed wire inside or outside the second laser beam. In this application, feeding powder inside the first laser beam and feeding wire inside the second laser beam are taken as an example. Using two beams can increase the total energy of the beams, thereby improving the cladding effect.

[0061] Fourth embodiment:

[0062] Reference Figure 5 and Figure 6 In the fourth embodiment, the powder feeder in step 2 includes a shell 1, a plurality of powder feeding tubes 2 are installed on the shell 1, a powder feeding port 11 is formed on the lower side of the shell 1, and the powder feeding port 11 is connected to the powder feeding channel of the laser cladding head. A quantitative mixing mechanism 3 is arranged in the shell 1 for quantitatively mixing a plurality of powders.

[0063] The quantitative mixing mechanism 3 includes a material receiving plate 31, a quantitative plate 32 and a material leakage plate 33. The material receiving plate 31 is fixedly installed in the housing 1. The material receiving plate 31 is provided with partitions 4 at intervals. The partitions 4 divide the material receiving plate 31 into a plurality of material receiving areas 41. The material receiving plate 31 is located in the material receiving area 41 and is provided with material receiving holes 311. All the material receiving holes 311 are arranged on the material receiving plate 31 in a circle. The material receiving plate 31 is located on the side of the material receiving holes 311 and has an arc surface formed thereon, so that the powder can be gathered at the material receiving holes 311. The number of the powder feeding pipes 2 is the same as the number of the material receiving holes 311. The powder enters the corresponding material receiving area 41 from the powder feeding pipe 2 and is gathered at the corresponding material receiving hole 311. In another embodiment, the material receiving hole 311 may be truncated cone-shaped, and the larger end of the material receiving hole 311 is located on the upper surface of the material receiving plate 31.

[0064] The quantitative disk 32 is rotatably connected in the shell 1, and the quantitative disk 32 is located below the receiving disk 31. A plurality of material receiving holes 321 are opened on the circumference of the receiving disk 31, and the number of the material receiving holes 321 is twice the number of the receiving holes 311. The leakage disk 33 is fixedly installed in the shell 1, and the leakage disk 33 is located below the quantitative disk 32. A plurality of material leakage holes 331 are opened on the circumference of the leakage disk 33, and the number of the leakage holes 331 is the same as the number of the receiving holes 311. All the leakage holes 331 and all the receiving holes 311 on the leakage disk 33 are staggered.

[0065] In the initial state, half of the material receiving holes 321 on the quantitative disk 32 will be connected with all the material receiving holes 311 on the material receiving disk 31, and the material leakage holes 331 on the leakage disk 33 are staggered with the material receiving holes 311. The powder falls into the material receiving holes 321 from the material receiving holes 311, and then the quantitative disk 32 rotates, and the remaining half of the material receiving holes 321 on the quantitative disk 32 are connected with the material receiving holes 311. After all the material receiving holes 321 filled with powder rotate, they correspond to and connect with all the leakage holes 331 one by one, and the powder leaks out from the leakage holes 331. Among them, the quantitative disk 32 can quantitatively feed the powder, and the feeding amount of different powders can be controlled. By setting the sizes of the material receiving holes 311 to different, it can be ensured that the proportion of powder falling into the material receiving holes 321 at the same time is different, so that the quantitative feeding of the powder is realized, and finally falls under the shell 1.

[0066] Reference Figure 5 and Figure 7 The quantitative mixing mechanism 3 also includes a rubber spring 34, which is located below the leakage tray 33. The rubber spring 34 is in a truncated cone shape, and the smaller end of the rubber spring 34 is located on the side away from the leakage tray 33. The shell 1 is located on the lower side of the rubber spring 34 and is arranged in a funnel shape.

[0067] When the powder falls from the leakage plate 33 onto the rubber dome 34 , the powder will bounce on the rubber dome 34 and toward the central axis of the rubber dome 34 . After the different powders bounce up, they will converge at the central axis of the rubber dome 34 to form a mixture and finally leak out from the smaller end of the rubber dome 34 .

[0068] A driving motor 5 is installed on the housing 1, and the output shaft of the driving motor 5 passes through the housing 1 and is connected to the quantitative disk 32. The driving motor 5 drives the quantitative disk 32 to rotate intermittently. A driving rod 6 is fixedly installed on the lower side of the quantitative disk 32, and the driving rod 6 is vertically arranged. A connecting rod 7 is installed at the larger side port of the rubber spring 34. The driving rod 6 and the connecting rod 7 are connected, that is, when the quantitative disk 32 rotates, the rubber spring 34 will be driven to rotate synchronously.

[0069] The driving motor 5 is operated and intermittently rotated, driving the quantitative disk 32 to intermittently rotate, thereby realizing intermittent material discharge. At the same time, the rubber spring 34 is intermittently rotated. When the powder falls on the rubber spring 34, the distributed powder adheres to the rubber spring 34 and cannot slide off. When the rubber spring 34 rotates, centrifugal force is generated so that the powder can slide off the rubber spring 34, thereby ensuring the material discharge effect.

[0070] The implementation principle of a laser cladding online metallurgical process in the embodiment of the present application is as follows: when laser cladding work is required for a corresponding substrate, if the corresponding powder is lacking, wire can be used as a substitute, and there is no need to produce powder, which helps to reduce the actual cost while performing the cladding work; with arc welding, it can help prevent the high reflectivity of the wire to the laser beam, resulting in poor cladding effect; the laser beam output is in a diamond shape, and the length direction of the wire is perpendicular to the first beam, which reduces energy damage, and after the second beam is shot onto the wire, the reflected beam will preheat the surface of the substrate, which is convenient for subsequent cladding work;

[0071] During the powder feeding process, the quantitative mixing mechanism 3 is used to achieve a fixed-proportion mixing of the powders and achieve uniform mixing, which helps to improve the performance of the substrate after cladding.

[0072] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A laser cladding online metallurgical process, characterized in that: Here are the steps: S1: Clean the required cladding area on the substrate surface; S2: adding wire to the surface of the substrate, and adding powder to the surface of the substrate at the same time, the powder is the alloy component missing in the wire, and using the first laser beam to clad the wire and the powder on the surface of the substrate; S3: forming a coating, which combines with the substrate surface after cooling; S4: Surface treatment of the coating; In step S2, powder material is added to the surface of the substrate by using a powder feeder, the powder feeder comprising a shell (1), a plurality of powder feeding tubes (2) are mounted on the shell (1), a powder feeding port (11) is formed on the lower side of the shell 1, the powder feeding port (11) is connected to the powder feeding channel of the laser cladding head, and a quantitative mixing mechanism (3) is arranged in the shell 1 for quantitatively mixing a plurality of powder materials; The quantitative mixing mechanism 3 comprises a material receiving plate (31), a quantitative plate (32) and a material leakage plate (33). The material receiving plate (31) is fixedly mounted in the housing 1. Partition plates (4) are installed at intervals on the material receiving plate (31). The partition plates (4) divide the material receiving plate (31) into a plurality of material receiving areas (41). The material receiving plate (31) is provided with material receiving holes (311) extending through the material receiving areas (41). All the material receiving holes (311) are arranged circumferentially on the material receiving plate (31). The material receiving plate (31) is provided with an arc surface on the circumference of the material receiving holes (311), so that the powder can be gathered at the material receiving holes (311). The number of the powder feeding pipes (2) is equal to the number of the material receiving holes (311). The quantitative disk (32) is rotatably connected in the housing (1), and the quantitative disk (32) is located below the material receiving disk (31). The material receiving disk (31) is provided with a plurality of material receiving holes (321) on its circumference, and the number of the material receiving holes (321) is twice the number of the material receiving holes (311). The leakage disk (33) is fixedly installed in the housing (1), and the leakage disk (33) is located below the quantitative disk (32). The leakage disk (33) is provided with a plurality of material leakage holes (331) on its circumference, and the number of the material leakage holes (331) is the same as the number of the material receiving holes (311). All the leakage holes (331) and all the material receiving holes (311) on the leakage disk (33) are staggered. The quantitative mixing mechanism (3) further comprises a rubber spring (34), the rubber spring (34) being located below the material leakage disc (33), the rubber spring (34) being in the shape of a truncated cone, the smaller end of the rubber spring (34) being located on a side away from the material leakage disc (33), and the housing 1 being located below the rubber spring (34) and arranged in the shape of a funnel.

2. The laser cladding online metallurgical process according to claim 1, characterized in that: In step S2, powder is coaxially fed within the first laser beam, and wire is fed outside the first laser beam.

3. The laser cladding online metallurgical process according to claim 2, characterized in that: In step S2, arc welding is used to melt and weld the wire material during wire feeding.

4. The laser cladding online metallurgical process according to claim 1, characterized in that: In step S2, wire is coaxially fed within the first laser beam, and powder is fed outside the first laser beam.

5. The laser cladding online metallurgical process according to claim 1, characterized in that: In step S2, powder is fed inside or outside the first laser beam, and a second laser beam is also used to feed wire inside or outside the second laser beam.

6. The laser cladding online metallurgical process according to claim 2, characterized in that: In step S2, if there are two bundles of wire, the two bundles of wire can be twisted to form a pair of twisted wires. If there are multiple bundles of wire, multiple twisted wires can be formed, and then the wires are transported.

Citation Information

Patent Citations

  • Wire-powder cooperation and laser-electric arc composite additive manufacturing device and method

    CN113385821A