Electrolytic copper foil for lithium battery and preparation method and application thereof

By adding specific additives and process control in the preparation process of electrolytic copper foil of lithium batteries, the problem of insufficient tensile strength attenuation and thermal stability of electrolytic copper foil at high temperatures is solved, and electrolytic with high thermal stability and high tensile performance is achieved Copper foil preparation.

CN118292056BActive Publication Date: 2024-11-26GUANGDONG YINGHUA ELECTRONIC TECH CO LTD

Patent Information

Application Number
CN202410408301.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-09-13
Filing Date
2024-04-07
Publication Date
2024-11-26
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

The existing electrolytic copper foil for lithium batteries has a large tensile strength attenuation under high temperature conditions, which is prone to fracture due to deformation, and lacks thermal stability, which cannot meet production needs.

Method used

Electrolysis with high thermal stability is prepared by adding a specific proportion of brightener, wetting agent and leveling agent to the electrolyte and performing coordinated control during the process, including electrolytic preparation, water washing, passivation treatment and annealing treatment. Copper foil.

Benefits of technology

Improve the thermal stability of electrolytic copper foil, avoid breakage caused by heat sources or deformation, high tensile strength and elongation at room temperature, and the tensile strength can still reach more than 90% of the room temperature after high temperature, and the surface does not have oxidation and discoloration, and the thermal stability Significantly improved sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004778238880000101
    Figure BDA0004778238880000101
  • Figure BDA0004778238880000111
    Figure BDA0004778238880000111
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrolytic copper foil, and specifically discloses an electrolytic copper foil for lithium batteries, a preparation method thereof, and an application thereof. The preparation method of the electrolytic copper foil comprises the preparation of an electrolyte, electrolytic preparation of raw foil, a first water washing, a surface passivation treatment of the raw foil, a second water washing, and an annealing treatment. The preparation of the electrolyte requires additives, and the additives include a brightener, a wetting agent, and a leveling agent. The electrolytic copper foil can remove the internal stress of the electrolytic copper foil in advance through the coordinated control of the proportion of the additives and the various parameters in the process steps, so that the grains are evenly and densely distributed, and the high warping of the electrolytic copper foil and the breakage of the electrolytic copper foil caused by subsequent heat sources or deformation are avoided, and the electrolytic copper foil has high thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrolytic copper foil, and in particular relates to an electrolytic copper foil for lithium batteries and a preparation method and application thereof. Background Art

[0002] Electrolytic copper foil is widely used in various fields such as printed circuit boards and negative electrode collectors of lithium-ion secondary batteries. As the negative electrode current collector of lithium batteries, electrolytic copper foil supports the negative electrode active materials in lithium batteries and collects and conducts electrons passing through the negative electrode materials of lithium batteries. Electrolytic copper foil will bring huge market demand with the development of lithium batteries in new energy, consumer electronics, energy storage and other fields.

[0003] In the process of preparing lithium batteries, electrolytic copper foil needs to go through the steps of surface coating of negative electrode materials, lamination, cutting, encapsulation, etc., and when the electrolytic copper foil is made into a lithium battery, the negative electrode material of the lithium battery will expand and shrink during the charging and discharging process to produce deformation and transfer the deformation to the electrolytic copper foil. These processes require the electrolytic copper foil for lithium batteries to have good tensile strength and elongation to avoid wrinkles and cracks in the electrolytic copper foil. At the same time, in order to make the negative electrode active material that is easy to deform during the charging and discharging process firmly bonded with the negative electrode current collector, an adhesive is usually required. During the curing process of the adhesive, the electrolytic copper foil will be subjected to high temperature hot pressing at about 200°C for 1-2 hours. If the tensile strength of the electrolytic copper foil is reduced too much after high temperature, the electrolytic copper foil is easily broken by the stress transmitted by the deformation of the negative electrode material, thereby increasing the qualified rate of lithium batteries and the safety during use.

[0004] Chinese patent CN101426959B discloses an electrolytic copper foil, a surface-treated copper foil using the electrolytic copper foil, a copper-clad laminate using the surface-treated copper foil, and a method for manufacturing the electrolytic copper foil. The electrolytic copper foil is manufactured by electrolysis using a sulfuric acid-based copper electrolyte containing a compound having a structure with a sulfonic acid group combined with a benzene ring, a sulfonate of an active sulfur compound, and a quaternary ammonium salt polymer having a ring structure. The electrolytic copper foil has a low-profile and glossy surface, and has a normal tensile strength value of 70 kgf / mm 2 -100kgf / mm 2The extremely high mechanical strength, after heating (180℃×60 minutes), also has a tensile strength value of more than 85% of the normal tensile strength value. Chinese patent CN104955988B discloses an electrolytic copper foil, a method for manufacturing the electrolytic copper foil, and a surface-treated copper foil obtained by using the electrolytic copper foil. The electrolytic copper foil is electrolyzed with a sulfuric acid copper electrolyte containing polyethyleneimine with a molecular weight of 10000-70000 at a concentration of 20mg / L-100mg / L and a chlorine concentration of 0.5mg / L-2.5mg / L, and has a normal tensile strength of more than 600MPa and a tensile strength of more than 470MPa after heating at 350℃ for 1 hour. The above-mentioned electrolytic copper foil has thermal stability, but in the preparation of electrolytic copper foil for lithium batteries below 6μm, the room temperature elongation is low, and after being heated, the tensile strength decays by more than 10%, and the thermal stability cannot meet the production requirements.

[0005] Currently, there is an urgent need for a production process for electrolytic copper foil for lithium batteries that has thermal stability and avoids high warping of the electrolytic copper foil and subsequent heat sources or deformation that cause the electrolytic copper foil to break. Summary of the invention

[0006] As used herein, the singular forms "a," "an," and "the" include both singular and plural referents unless the context clearly dictates otherwise. Numerical ranges recited by endpoints include all numbers and fractions within the corresponding ranges, as well as the recited endpoints.

[0007] In view of the problems existing in the prior art, the present invention provides an electrolytic copper foil for lithium batteries and a preparation method and application thereof. By means of specific production additives and their specific proportions as well as coordinated control between various processes, the thermal stability of the electrolytic copper foil can be improved, and the high warping of the electrolytic copper foil and the breakage of the electrolytic copper foil caused by subsequent heat sources or deformation can be avoided.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0009] The present invention provides a method for preparing an electrolytic copper foil for a lithium battery, comprising the following steps:

[0010] S1. Preparation of electrolyte: After copper and sulfuric acid are mixed to obtain a primary copper sulfate electrolyte, add Cl - Mixing to obtain a secondary electrolyte, and then mixing with an additive to obtain an electrolyte after maintaining a high temperature;

[0011] S2. Electrolytic preparation of green foil: electrolytic preparation of green foil in an electrolyte;

[0012] S3, first water washing: washing with water to remove excess electrolyte on the surface of the raw foil;

[0013] S4, raw foil surface passivation treatment: passivating the raw foil after the first water washing with a passivation solution;

[0014] S5, second water washing: washing with water to remove excess passivation liquid on the surface of the raw foil;

[0015] S6, annealing treatment: drying and rolling the raw foil after the second water washing, and then heating, keeping the temperature and then cooling down in a nitrogen atmosphere to obtain the electrolytic copper foil;

[0016] Preferably, the additives in step S1 include brighteners, wetting agents and leveling agents.

[0017] Preferably, the brightener comprises sodium thiazoline dithiopropane sulfonate and / or sodium 3-mercapto-1-propane sulfonate; the wetting agent comprises hydroxyethyl cellulose and / or polyethylene glycol; and the leveling agent comprises 1,1-dimethylpropargylamine and / or agarose.

[0018] Preferably, the mass ratio of the brightener, the wetting agent and the leveling agent is 0.1-1:2:1.

[0019] Further preferably, the mass ratio of the brightener, the wetting agent and the leveling agent is 1:2:1.

[0020] Preferably, the concentration of sodium thiazolyl dithiopropane sulfonate in the brightener is 16-20 mg / L; the concentration of sodium 3-mercapto-1-propane sulfonate is 8-10 mg / L; the concentration of hydroxyethyl cellulose in the wetting agent is 24-30 mg / L; the concentration of polyethylene glycol is 24-30 mg / L; the concentration of 1,1-dimethylpropargylamine in the leveling agent is 12-16 mg / L; and the concentration of agarose is 12-14 mg / L.

[0021] Preferably, the high temperature in step S1 is 49°C-51°C.

[0022] Preferably, the electrolyte in step S1 contains Cu 2+ The concentration of 90-110g / L, the concentration of sulfuric acid is 110-130g / L, and the concentration of Cl - The concentration is 15-20mg / L.

[0023] Preferably, the copper in step S1 includes copper wire, copper block, copper powder or copper rod.

[0024] Preferably, the electrolysis conditions in step S2 are: temperature 49°C-51°C, current density 60-70A / dm 2 .

[0025] Preferably, the conditions for water washing in step S3 and step S5 are: the water is RO water, the temperature is 25° C.-35° C., and the flow rate is 1-2 L / min.

[0026] Preferably, the passivation solution in step S4 comprises chromic anhydride, glucose and purified water.

[0027] Preferably, the passivation treatment conditions in step S4 are: the pH of the passivation solution is 3.0-3.6, the temperature is 30°C-35°C, and the current density is 1-3A / dm 2 .

[0028] Preferably, the insulation temperature in step S6 is 110° C.-120° C., and the insulation time is 3 h-5 h.

[0029] The present invention also provides an electrolytic copper foil prepared by the above-mentioned preparation method.

[0030] The present invention also provides an application of the electrolytic copper foil or the electrolytic copper foil prepared by the above preparation method in preparing lithium batteries.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The electrolytic copper foil prepared by the present invention has high thermal stability. Through specific production additives and their specific proportions as well as coordinated control between various processes, the internal stress of the electrolytic copper foil can be removed in advance, so that the grains are evenly and densely distributed, and the high warping degree of the electrolytic copper foil and the subsequent heat source or deformation caused by the electrolytic copper foil are avoided. The electrolytic copper foil of the present invention has high room temperature tensile strength and elongation. After high temperature heating, the tensile strength can still reach more than 90% of the room temperature tensile strength, and there is no oxidation discoloration on the surface, and the thermal stability is high. DETAILED DESCRIPTION

[0033] The present invention is described below through specific embodiments to make the technical solution of the present invention easier to understand and grasp, but the present invention is not limited thereto, and the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments.

[0034] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0035] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention. The experimental methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0036] Example 1 A method for preparing electrolytic copper foil for lithium batteries

[0037] Step 1: Preparation of electrolyte. Put copper wire in the copper dissolving tank, add sulfuric acid from the top of the copper wire to the bottom, and use a blower to blow high-temperature air from the bottom to the top of the copper wire to obtain a first-level copper sulfate electrolyte; after filtering the first-level copper sulfate electrolyte, add Cl - The secondary electrolyte is mixed to obtain the secondary electrolyte; the secondary electrolyte is maintained at a temperature of 49-51°C through a heat exchanger, and then transported to a high-level tank and mixed evenly with 434kg of additives to obtain 40m 3 The electrolyte can be used for electrolysis by pumping the electrolyte into the electrolytic cell.

[0038] The additives are composed of a brightener, a wetting agent and a leveling agent, and the brightener, the wetting agent and the leveling agent are present in the electrolyte in a mass ratio of 1:2:1.

[0039] Among them, the brightener has the effect of refining grains, and is composed of 16 mg / L of sodium thiazoline dithiopropane sulfonate and 8 mg / L of sodium 3-mercapto-1-propane sulfonate; the wetting agent can reduce the surface tension of the electrolyte and make the coating crystallized and dense, and is composed of 24 mg / L of hydroxyethyl cellulose and 24 mg / L of polyethylene glycol. The leveling agent can smooth the microscopic contour of the copper foil surface and reduce the surface roughness, and is composed of 12 mg / L of 1,1-dimethylpropargylamine and 12 mg / L of agarose.

[0040] The electrolyte contains 100 g / L Cu 2+ , 120g / L H2SO 4、 15mg / L Cl - , and the solvent in the electrolyte is ultrapure water.

[0041] Step 2: Electrolytic preparation of green foil at 49-51°C and 65A / dm 2 The raw foil is prepared by electrolysis in an electrolytic cell at a current density of .

[0042] Step 3, first water washing: water washing is used to remove excess electrolyte on the surface of the raw foil. The washing water used is RO water with a temperature of 30°C and a flow rate of 2L / min.

[0043] Step 4: Surface passivation of raw foil. The prepared raw foil is subjected to conventional passivation treatment to obtain uncut finished electrolytic copper foil for lithium battery. The conventional passivation treatment uses a passivation solution containing 110 mg / L chromic anhydride, 220 mg / L glucose and RO water, the pH of the passivation solution is 3.0, the passivation treatment temperature is 32°C, and the passivation treatment current is 2A / dm 2 .

[0044] Step 5, second water washing: water washing is used to remove excess passivation liquid on the surface of the raw foil. RO water is used for water washing, the temperature is 30°C, and the flow rate is 2L / min.

[0045] Step 6: Drying: The oven temperature is 110°C to remove the residual washing water on the surface of the electrolytic copper foil.

[0046] Step 7: Roll up.

[0047] Step 8, annealing treatment: put the electrolytic copper foil into a heating furnace with a nitrogen atmosphere, heat it to 110°C at a rate of 1°C / min, keep it warm for 5 hours, and then cool it to room temperature with the furnace to obtain the uncut finished electrolytic copper foil.

[0048] Example 2 A method for preparing electrolytic copper foil for lithium battery

[0049] Step 1: Preparation of electrolyte. Put a copper block in a copper dissolving tank, add sulfuric acid from the top of the copper block to the bottom, and use a blower to blow high-temperature air from the bottom to the top of the copper block to obtain a first-level copper sulfate electrolyte; after filtering the first-level copper sulfate electrolyte, add Cl - The secondary electrolyte is mixed to obtain the secondary electrolyte; the secondary electrolyte is maintained at a temperature of 49-51°C through a heat exchanger, and then transported to a high-level tank and mixed evenly with 434kg of additives to obtain 40m 3 The electrolyte can be used for electrolysis by pumping the electrolyte into the electrolytic cell.

[0050] The additives are composed of a brightener, a wetting agent and a leveling agent, and the brightener, the wetting agent and the leveling agent are present in the electrolyte at a mass ratio of 0.5:2:1.

[0051] Among them, the brightener has the effect of refining grains, and is composed of 20 mg / L of sodium thiazoline dithiopropane sulfonate and 10 mg / L of sodium 3-mercapto-1-propane sulfonate; the wetting agent can reduce the surface tension of the electrolyte and make the coating crystallized and dense, and is composed of 30 mg / L of hydroxyethyl cellulose and 30 mg / L of polyethylene glycol. The leveling agent can smooth the microscopic contour of the copper foil surface and reduce the surface roughness, and is composed of 16 mg / L of 1,1-dimethylpropargylamine and 14 mg / L of agarose.

[0052] The electrolyte contains 90 g / L of Cu 2+ , 110g / L H2SO 4、 18mg / L Cl - , and the solvent in the electrolyte is ultrapure water.

[0053] Step 2: Electrolytic preparation of green foil at 49-51°C and 60A / dm 2 The raw foil is prepared by electrolysis in an electrolytic cell at a current density of .

[0054] Step 3: First water washing: Wash with water to remove excess electrolyte on the surface of the raw foil. The washing water used is RO water with a temperature of 25°C and a flow rate of 2L / min.

[0055] Step 4: Surface passivation of raw foil. The prepared raw foil is subjected to conventional passivation treatment to obtain uncut finished electrolytic copper foil for lithium battery. The conventional passivation treatment uses a passivation solution containing 110 mg / L chromic anhydride, 220 mg / L glucose and RO water, the pH of the passivation solution is 3.4, the passivation treatment temperature is 30°C, and the passivation treatment current is 1A / dm 2 .

[0056] Step 5, second water washing: water washing is used to remove excess passivation liquid on the surface of the raw foil. RO water is used for water washing, the temperature is 25°C, and the flow rate is 1.5L / min.

[0057] Step 6: Drying: The oven temperature is 105°C to remove the residual washing water on the surface of the electrolytic copper foil.

[0058] Step 7: Roll up.

[0059] Step 8, annealing treatment: put the electrolytic copper foil into a heating furnace with a nitrogen atmosphere, heat it to 115°C at a rate of 1°C / min, keep it warm for 4 hours, and then cool it to room temperature with the furnace to obtain the uncut finished electrolytic copper foil.

[0060] Example 3 A method for preparing electrolytic copper foil for lithium battery

[0061] Step 1: Preparation of electrolyte. Put copper powder in a copper dissolving tank, add sulfuric acid from the top of the copper powder to the bottom, and blow high-temperature air from the bottom of the copper powder to the top with a blower to obtain a first-level copper sulfate electrolyte; after filtering the first-level copper sulfate electrolyte, add Cl - The secondary electrolyte is mixed to obtain the secondary electrolyte; the secondary electrolyte is maintained at a temperature of 49-51°C through a heat exchanger, and then transported to a high-level tank and mixed evenly with 434kg of additives to obtain 40m 3 The electrolyte can be used for electrolysis by pumping the electrolyte into the electrolytic cell.

[0062] The additives are composed of a brightener, a wetting agent and a leveling agent, and the brightener, the wetting agent and the leveling agent are present in the electrolyte at a mass ratio of 0.1:2:1.

[0063] Among them, the brightener has the effect of refining grains, and is composed of 18 mg / L of sodium thiazoline dithiopropane sulfonate and 9 mg / L of sodium 3-mercapto-1-propane sulfonate; the wetting agent can reduce the surface tension of the electrolyte and make the coating crystallized and dense, and is composed of 26 mg / L of hydroxyethyl cellulose and 26 mg / L of polyethylene glycol. The leveling agent can smooth the microscopic contour of the copper foil surface and reduce the surface roughness, and is composed of 14 mg / L of 1,1-dimethylpropargylamine and 13 mg / L of agarose.

[0064] The electrolyte contains 110 g / L of Cu 2+ , 130g / L H2SO 4、 20mg / L Cl - , and the solvent in the electrolyte is ultrapure water.

[0065] Step 2: Electrolytic preparation of green foil at 49-51°C and 70A / dm 2 The raw foil is prepared by electrolysis in an electrolytic cell at a current density of .

[0066] Step 3, first water washing: water washing to remove excess electrolyte on the surface of the raw foil. The washing water used is RO water with a temperature of 35°C and a flow rate of 2L / min.

[0067] Step 4: Surface passivation of raw foil. The prepared raw foil is subjected to conventional passivation treatment to obtain uncut finished electrolytic copper foil for lithium battery. The conventional passivation treatment uses a passivation solution containing 110 mg / L chromic anhydride, 220 mg / L glucose and RO water, the pH of the passivation solution is 3.6, the passivation treatment temperature is 35°C, and the passivation treatment current is 3A / dm 2 .

[0068] Step 5, second water washing: water washing is used to remove excess passivation liquid on the surface of the raw foil. RO water is used for water washing, the temperature is 35°C, and the flow rate is 1L / min.

[0069] Step 6: Drying: The oven temperature is 115°C to remove the residual washing water on the surface of the electrolytic copper foil.

[0070] Step 7: Roll up.

[0071] Step 8, annealing treatment: put the electrolytic copper foil into a heating furnace with a nitrogen atmosphere, heat it to 120°C at a rate of 1°C / min, keep it warm for 3 hours, and then cool it to room temperature with the furnace to obtain the uncut finished electrolytic copper foil.

[0072] Comparative Example 1: A method for preparing electrolytic copper foil for lithium batteries

[0073] The difference from Example 1 is that:

[0074] The brightener, wetting agent and leveling agent in the additive in step 1 are present in the electrolyte at a mass ratio of 2:2:1. The brightener is composed of 16 mg / L sodium thiazoline dithiopropane sulfonate and 8 mg / L sodium 3-mercapto-1-propane sulfonate; the wetting agent is composed of 12 mg / L hydroxyethyl cellulose and 12 mg / L polyethylene glycol; the leveling agent is composed of 12 mg / L 1,1-dimethylpropargylamine and 12 mg / L agarose.

[0075] The other steps are the same as those in Example 1.

[0076] Comparative Example 2: A method for preparing electrolytic copper foil for lithium batteries

[0077] The difference from Example 1 is that:

[0078] The brightener, wetting agent and leveling agent in the additive in step 1 are present in the electrolyte in a mass ratio of 1:2:1. The brightener is composed of 12 mg / L of sodium thiazoline dithiopropane sulfonate and 12 mg / L of sodium 3-mercapto-1-propane sulfonate. The wetting agent is composed of 24 mg / L of hydroxyethyl cellulose and 24 mg / L of polyethylene glycol. The leveling agent is composed of 12 mg / L of 1,1-dimethylpropargylamine and 12 mg / L of agarose.

[0079] The other steps are the same as those in Example 1.

[0080] Comparative Example 3: A method for preparing electrolytic copper foil for lithium batteries

[0081] The difference from Example 1 is that:

[0082] The brightener, wetting agent and leveling agent in the additive in step 1 are present in the electrolyte in a mass ratio of 1:2:1. The brightener is composed of 16 mg / L of sodium polydisulfide dipropane sulfonate and 8 mg / L of sodium 3-mercapto-1-propane sulfonate. The wetting agent is composed of 24 mg / L of hydroxyethyl cellulose and 24 mg / L of polyethylene glycol. The leveling agent is composed of 12 mg / L of acid copper strong leveling agent (POSS) and 12 mg / L of agarose.

[0083] The other steps are the same as those in Example 1.

[0084] Comparative Example 4: A method for preparing electrolytic copper foil for lithium batteries

[0085] The difference from Example 1 is that:

[0086] In step 1, a step of annealing the copper wire is added, and then the electrolyte is prepared: the copper wire is placed in a heating furnace with a nitrogen atmosphere, and the temperature is raised to 110°C at a rate of 1°C / min. After being kept warm for 5 hours, it is cooled to room temperature with the furnace for annealing.

[0087] After step 7, the uncut finished electrolytic copper foil is obtained after the coiling, and the annealing treatment in step 8 is not required.

[0088] The other steps are the same as those in Example 1.

[0089] Comparative Example 5: A method for preparing electrolytic copper foil for lithium batteries

[0090] The difference from Example 1 is that:

[0091] In the annealing treatment in step 8, the electrolytic copper foil is placed in a heating furnace with a nitrogen atmosphere, and the temperature is raised to 130° C. at a rate of 1° C. / min. After being kept at this temperature for 5 hours, the foil is cooled to room temperature along with the furnace, and an uncut finished electrolytic copper foil is obtained.

[0092] The other steps are the same as those in Example 1.

[0093] Effect example

[0094] Referring to the test method in GB / T 29847-2013, the thickness, warpage, room temperature tensile strength and room temperature tensile elongation of the electrolytic copper foil were tested. The electrolytic copper foil was placed in a conventional drying oven and baked at 200°C for 2 hours. The tensile strength and tensile elongation were tested in accordance with the method in GB / T29847-2013, that is, the tensile strength after baking at 200°C for 2 hours and the tensile elongation after baking at 200°C for 2 hours were obtained. The oxidation resistance test was to place the electrolytic copper foil in a conventional oven, bake it at 140°C for 15 minutes, and observe whether there was any oxidation discoloration on the surface of the electrolytic copper foil. According to the above test methods, the physical properties of the electrolytic copper foils of Examples 1-3 and Comparative Examples 1-5 were measured respectively.

[0095] Table 1 Physical properties of electrolytic copper foil

[0096]

[0097]

[0098] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing an electrolytic copper foil for a lithium battery, characterized in that: The following steps are involved: S1. Preparation of electrolyte: After copper and sulfuric acid are mixed to obtain a primary copper sulfate electrolyte, add Cl - Mixing to obtain a secondary electrolyte, and then mixing with an additive to obtain an electrolyte after maintaining a high temperature; S2. Electrolytic preparation of green foil: electrolytic preparation of green foil in an electrolyte; S3, first water washing: washing with water to remove excess electrolyte on the surface of the raw foil; S4, raw foil surface passivation treatment: passivating the raw foil after the first water washing with a passivation solution; S5, second water washing: washing with water to remove excess passivation liquid on the surface of the raw foil; S6, annealing treatment: drying and rolling the raw foil after the second water washing, and then heating, keeping the temperature and then cooling down in a nitrogen atmosphere to obtain the electrolytic copper foil; The high temperature in step S1 is 49°C-51°C; The additives in step S1 include a brightener, a wetting agent and a leveling agent, and the mass ratio of the brightener, the wetting agent and the leveling agent is 0.1-1:2:1; The concentration of sodium thiazoline dithiopropane sulfonate in the brightener is 16-20 mg / L, and the concentration of sodium 3-mercapto-1-propane sulfonate is 8-10 mg / L; the concentration of hydroxyethyl cellulose in the wetting agent is 24-30 mg / L, and the concentration of polyethylene glycol is 24-30 mg / L; the concentration of 1,1-dimethylpropargylamine in the leveling agent is 12-16 mg / L, and the concentration of agarose is 12-14 mg / L.

2. The preparation method according to claim 1, characterized in that: The electrolyte in step S1 contains Cu 2+ The concentration of 90-110g / L, the concentration of sulfuric acid is 110-130g / L, and the concentration of Cl - The concentration is 15-20mg / L.

3. The preparation method according to claim 1, characterized in that: The electrolysis conditions in step S2 are: temperature 49°C-51°C, current density 60-70A / dm 2 ; The insulation temperature in step S6 is 110℃-120℃, and the insulation time is 3h-5h.

4. The preparation method according to claim 1, characterized in that: The conditions for water washing in step S3 and step S5 are: the water is RO water, the temperature is 25°C-35°C, and the flow rate is 1-2 L / min.

5. The preparation method according to claim 1, characterized in that: The passivation solution in step S4 includes chromic anhydride, glucose and purified water; the passivation treatment conditions in step S4 are: the pH of the passivation solution is 3.0-3.6, the temperature is 30°C-35°C, and the current density is 1-3A / dm 2 .

6. An electrolytic copper foil, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the electrolytic copper foil according to claim 6 or the electrolytic copper foil prepared by the preparation method according to any one of claims 1 to 5 in preparing lithium batteries.

Citation Information

Patent Citations

  • Electrolytic copper foil, surface treated copper foil using the electrolytic copper foil, copper-clad laminated plate using the surface treated copper foil, and method for manufacturing the electrolyt

    CN101426959B

  • Electrolytic copper foil, a method for manufacturing the electrolytic copper foil, and a surface-treated copper foil obtained from the electrolytic copper foil.

    CN104955988B

  • Electrolyte for preparing high-tensile lithium battery copper foil

    CN108677224A

  • High-tensile-strength copper foil, manufacturing method and system thereof

    CN111041530A

  • Copper foil additive for fifth-generation mobile communication board, copper foil and production process of copper foil

    CN111394754A

Cited By

  • Electrolyte and preparation method of electrolytic copper foil for lithium battery

    CN120366861A

  • Preparation method of electrolyte and electrolytic copper foil for lithium batteries

    CN120366861B