A fire-retardant polymer material and preparation method thereof

By mixing and hot pressing polypropylene, diisopropylene peroxide and modified silver-loaded silica, the problem of flammability of polypropylene is solved, and efficient flame retardant performance and tensile strength are improved to ensure that The safety and antibacterial properties of the material are provided.

CN118325238BActive Publication Date: 2024-11-19SUZHOU HERUNCHANG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410761632.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-11-19
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

Polypropylene is flammable and melt drips when burning, which limits its widespread use and needs to improve its fire-retardant properties to improve safety performance.

Method used

The fire-resistant flame-retardant polymer materials are prepared by mixing and intensive refining of polypropylene, diapropylene peroxide and modified silver-carrying silica. The silver-carrying silica is improved by specific treatment methods such as extraction and activation treatment. The reactivity and dispersion of the crosslinking network structure is formed.

Benefits of technology

It significantly improves the tensile strength and flame retardant properties of the material, enhances the antibacterial effect, and ensures the safe performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a fire-retardant polymer material and a preparation method thereof, and relates to the technical field of polymer materials. When preparing the fire-retardant polymer material, the present invention uses hexadecyltrimethylammonium bromide as a template, hydrolyzes tetraethyl orthosilicate to obtain porous silica by self-polymerization, removes the template by extraction, and then vacuumizes and immerses it in a silver nitrate solution, and finally passes hydrogen chloride gas to obtain silver-loaded silica; after the silver-loaded silica is treated with tetraethyl orthosilicate, it is reacted with spirocyclic phosphate dichloride, allylphosphine dichloride, and 1,1,3,3-tetramethyl-1,3-disiloxane diol to obtain modified silver-loaded silica; polypropylene, diisopropylbenzene peroxide, and modified silver-loaded silica are mixed and kneaded, and then hot-pressed to obtain the fire-retardant polymer material. The fire-retardant polymer material prepared by the present invention has good tensile strength, antibacterial properties, and flame retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a fire-proof and flame-retardant polymer material and a preparation method thereof. Background Art

[0002] Polypropylene is one of the resins with the largest demand in the world. It has excellent properties such as high transparency, non-toxicity, easy processing, corrosion resistance, good mechanical properties, low price, and low density. It is widely used in the fields of construction, chemical industry, packaging, transportation, cables, electronics, etc. With the continuous expansion of the application of polypropylene, it can effectively replace other resins in many fields. For example, highly transparent polypropylene has become one of the important choices to replace polystyrene and polyvinyl chloride. In the fields of electrical appliances and furniture, the lightweight and ultra-thin development trend of polypropylene has become a strong competitor to replace metals and other materials.

[0003] However, since polypropylene is a non-charring polymer, it is very easy to burn, and there is also severe melting dripping during the combustion process. Therefore, polypropylene is very easy to cause fire and cause the fire to spread, which greatly limits its wide application. Based on the wide demand for polypropylene, it is very necessary to flame retard polypropylene to improve its safety performance. Summary of the invention

[0004] The purpose of the present invention is to provide a fire-retardant polymer material and a preparation method thereof to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] The invention discloses a fireproof and flame-retardant polymer material, which is obtained by hot pressing after mixing and kneading polypropylene, dicumyl peroxide and modified silver-carrying silicon dioxide.

[0007] As an optimization, the modified silver-loaded silica is prepared by treating the silver-loaded silica with tetraethyl orthosilicate and then reacting it with spirocyclic phosphate dichloride, allyl phosphine dichloride, and 1,1,3,3-tetramethyl-1,3-disiloxane diol.

[0008] As an optimization, the silver-loaded silica is prepared by hydrolyzing and self-polymerizing ethyl orthosilicate using hexadecyltrimethylammonium bromide as a template to obtain porous silica, removing the template by extraction, then vacuuming and immersing in a silver nitrate solution, and finally treating with hydrogen chloride gas.

[0009] A method for preparing a fire-retardant polymer material comprises the following preparation steps:

[0010] (1) 1 mol / L ammonia water, template agent and 20-30% ethanol aqueous solution are mixed in a mass ratio of 1:1:(45-55), stirred at 20-30°C and 800-1000 r / min for 30-40 min, and then added with stirring and tetraethyl orthosilicate solution. The ratio of the molar amount of tetraethyl orthosilicate to the molar amount of template agent in the tetraethyl orthosilicate solution is 4:1. The reaction is continued with stirring at 25-30°C for 8-10 h, and then the stirring is stopped and allowed to stand for 8-12 h. The porous silica is separated by centrifugation and washed with pure water for 3-5 times. The porous silica is dried at 70°C for 3-4 h to obtain the porous silica.

[0011] (2) Immerse the porous silica in the extracting solution, stir at 60-65°C and 200-300 r / min for 8-10 hours, centrifuge and wash with pure water for 3 times, and dry at 70°C for 3 hours to obtain the porous silica with the template removed; place the porous silica with the template removed in a container, adjust the pressure to 50 Pa with a vacuum pump, add 0.2 mol / L silver nitrate solution to immerse the porous silica with the template removed, ultrasonically disperse for 10 minutes, restore to normal pressure and stand for 30 minutes, centrifuge and place in a container, and pass hydrogen chloride gas at a rate of 1 mL / s for 30-40 minutes, then wash with pure water for 3-5 times and filter, dry at 70°C for 3 hours to obtain silver-loaded silica;

[0012] (3) activating the silver-loaded silica to obtain activated silver-loaded silica; mixing spirocyclic phosphate dichloride, allylphosphine dichloride, and 1,1,3,3-tetramethyl-1,3-disiloxanediol at a molar ratio of 0.5:0.5:1, adding 0.3-0.4 times the mass of spirocyclic phosphate dichloride activated silver-loaded silica, stirring and reacting at 20-30°C and 200-300 r / min for 60-80 min, heating to 85°C at a heating rate of 1°C / min and continuing stirring and reacting for 3-4 h, centrifuging and washing with anhydrous ethanol for 3-5 times to obtain modified silver-loaded silica;

[0013] (4) Weigh 90-100 parts of polypropylene, 0.3-0.4 parts of diisopropylbenzene peroxide, and 4-5 parts of modified silver-loaded silica according to their mass fractions; add the components into an internal mixer, mix at 180-190°C and 60-70 r / min for 10-12 min, hot press at 180-190°C and 12-15 MPa for 15-20 min, cool naturally to 100°C and keep warm for 6-8 h, and take out after cooling to room temperature to obtain a fire-retardant polymer material.

[0014] As an optimization, the template agent in step (1) is hexadecyltrimethylammonium bromide.

[0015] As an optimization, the tetraethyl orthosilicate solution in steps (1) and (3) is prepared by uniformly mixing tetraethyl orthosilicate and anhydrous ethanol in a mass ratio of 1:(8-10).

[0016] As an optimization, the extract in step (2) is prepared by uniformly mixing 1 mol / L hydrochloric acid aqueous solution and anhydrous ethanol in a volume ratio of 1:2.

[0017] As an optimization, the activation method in step (3) is as follows: silver-loaded silica, pure water and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(2-3):(8-10), stirred at 20-30°C and 600-800 r / min for 20-25 min, then 0.3-0.4 times the mass of the silver-loaded silica in a 1 mol / L sodium hydroxide solution and 2-3 times the mass of the silver-loaded silica in an ethyl orthosilicate solution are added, ultrasonicated at 20-30°C for 1-2 h, centrifuged and washed with anhydrous ethanol for 3-5 times, and dried at 60-70°C for 6-8 h.

[0018] As an optimization, the model of the polypropylene in step (3) is F401.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] When preparing the fireproof and flame-retardant polymer material, the present invention mixes polypropylene, dicumyl peroxide and modified silver-carrying silicon dioxide, performs internal kneading and hot pressing to obtain the fireproof and flame-retardant polymer material.

[0021] Firstly, hexadecyltrimethylammonium bromide is used as a template, and ethyl orthosilicate is hydrolyzed and self-polymerized to obtain porous silica. The template is removed by extraction, and then the mixture is vacuumized and immersed in a silver nitrate solution. Finally, silver-loaded silica is obtained by passing hydrogen chloride gas. The method of removing the template adopts an extraction method, which will not cause the collapse or blockage of the pores and can better load silver ions. The immersion method uses vacuumization to allow the silver nitrate solution to enter the pores through negative pressure, and better load, thereby improving the subsequent sterilization effect. Hydrogen chloride is used to convert the water-soluble silver nitrate into silver chloride to achieve a sustained release effect, making the antibacterial effect more lasting.

[0022] Secondly, the silver-loaded silica is treated with tetraethyl orthosilicate and then reacted with spirocyclic phosphate dichloride, allyl phosphine dichloride, and 1,1,3,3-tetramethyl-1,3-disiloxane diol to obtain modified silver-loaded silica. The silver-loaded silica is activated to make the surface have higher reactivity. After the modification, long silicon-phosphorus chains are generated on the surface of the silver-loaded silica, which improves the dispersibility, and the silicon-phosphorus elements coordinate flame retardancy, having good flame retardant effect; and the double bonds introduced into allyl phosphine dichloride can subsequently be initiated by diisopropyl peroxide and cross-linked with polypropylene to form a cross-linked network structure, thereby improving the tensile strength. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are described in detail.

[0025] Example 1

[0026] A method for preparing a fire-retardant polymer material, the method for preparing a fire-retardant polymer material mainly comprises the following preparation steps:

[0027] (1) Ethyl orthosilicate and anhydrous ethanol are mixed in a mass ratio of 1:8 to prepare an ethyl orthosilicate solution; 1 mol / L ammonia water, hexadecyltrimethylammonium bromide and 20-30% ethanol aqueous solution are mixed in a mass ratio of 1:1:45, stirred at 20°C and 800 r / min for 40 min, stirred continuously and added with the ethyl orthosilicate solution, the ratio of the molar amount of ethyl orthosilicate to the molar amount of hexadecyltrimethylammonium bromide in the ethyl orthosilicate solution is 4:1, stirred continuously at 25°C for 10 h, stopped stirring and allowed to stand for 8 h, centrifuged and washed with pure water 3 times, dried at 70°C for 3 h, and porous silica was obtained;

[0028] (2) 1 mol / L hydrochloric acid aqueous solution and anhydrous ethanol were mixed in a volume ratio of 1:2 to prepare an extract; the porous silica was immersed in the extract, stirred at 60°C and 200 r / min for 10 h, centrifuged and washed with pure water for 3 times, and dried at 70°C for 3 h to obtain the porous silica with the template removed; the porous silica with the template removed was placed in a container, the pressure was adjusted to 50 Pa with a vacuum pump, 0.2 mol / L silver nitrate solution was added to immerse the porous silica with the template removed, ultrasonically dispersed for 10 min, restored to normal pressure and allowed to stand for 30 min, centrifuged and placed in a container, and hydrogen chloride gas was introduced at a rate of 1 mL / s for 30 min, then washed with pure water for 3 times and filtered, and dried at 70°C for 3 h to obtain silver-loaded silica;

[0029] (3) Silver-loaded silica, pure water and anhydrous ethanol were mixed uniformly in a mass ratio of 1:2:8, stirred at 20°C and 600 r / min for 25 min, then 0.3 times the mass of the silver-loaded silica in a 1 mol / L sodium hydroxide solution and 2 times the mass of the silver-loaded silica in an ethyl orthosilicate solution were added, ultrasonicated at 20°C for 2 h, centrifuged and washed with anhydrous ethanol for 3 times, and dried at 60°C for 8 h to obtain activated silver-loaded silica; spirocyclic phosphate diacyl Chlorine, allylphosphine dichloride and 1,1,3,3-tetramethyl-1,3-disiloxanediol were uniformly mixed in a molar ratio of 0.5:0.5:1, activated silver-loaded silica in an amount of 0.3 times the mass of spirocyclic phosphate diacyl chloride was added, stirred at 20°C and 200 r / min for 80 min, heated to 85°C at a heating rate of 1°C / min and continued to stir for 3 h, centrifuged and washed 3 times with anhydrous ethanol to obtain modified silver-loaded silica;

[0030] (4) Weigh 90 parts of F401 polypropylene, 0.3 parts of diisopropylbenzene peroxide, and 4 parts of modified silver-loaded silica according to their mass fractions; add each component into an internal mixer, mix at 180°C, 60 r / min for 12 min, hot press at 180°C, 12 MPa for 20 min, cool naturally to 100°C and keep warm for 6 h, and take out after cooling to room temperature to obtain a fire-retardant polymer material.

[0031] Example 2

[0032] A method for preparing a fire-retardant polymer material, the method for preparing a fire-retardant polymer material mainly comprises the following preparation steps:

[0033] (1) Ethyl orthosilicate and anhydrous ethanol are mixed in a mass ratio of 1:9 to prepare an ethyl orthosilicate solution; 1 mol / L ammonia water, hexadecyltrimethylammonium bromide and a 25% ethanol aqueous solution are mixed in a mass ratio of 1:1:50, stirred at 25°C and 900 r / min for 35 minutes, stirred continuously and added with the ethyl orthosilicate solution, the ratio of the molar amount of ethyl orthosilicate to the molar amount of hexadecyltrimethylammonium bromide in the ethyl orthosilicate solution is 4:1, stirred continuously at 28°C for 9 hours, stopped stirring and allowed to stand for 10 hours, centrifuged and washed with pure water 4 times, dried at 70°C for 3.5 hours, and porous silica is obtained;

[0034] (2) 1 mol / L hydrochloric acid aqueous solution and anhydrous ethanol were mixed in a volume ratio of 1:2 to prepare an extracting solution; the porous silica was immersed in the extracting solution, stirred at 62°C and 250 r / min for 9 h, centrifuged and washed with pure water for 3 times, and dried at 70°C for 3 h to obtain the porous silica with the template removed; the porous silica with the template removed was placed in a container, the pressure was adjusted to 50 Pa with a vacuum pump, 0.2 mol / L silver nitrate solution was added to immerse the porous silica with the template removed, ultrasonically dispersed for 10 min, restored to normal pressure and allowed to stand for 30 min, centrifuged and placed in a container, and hydrogen chloride gas was introduced at a rate of 1 mL / s for 35 min, then washed with pure water 4 times and filtered, and dried at 70°C for 3 h to obtain silver-loaded silica;

[0035] (3) Silver-loaded silica, pure water and anhydrous ethanol were mixed uniformly in a mass ratio of 1:2.5:9, stirred at 25°C and 700 r / min for 22 min, then 0.35 times the mass of the silver-loaded silica in a 1 mol / L sodium hydroxide solution and 2.5 times the mass of the silver-loaded silica in an ethyl orthosilicate solution were added, ultrasonicated at 25°C for 1.5 h, centrifuged and washed with anhydrous ethanol for 4 times, and dried at 65°C for 7 h to obtain activated silver-loaded silica; spirocyclic phosphate Diacyl chloride, allylphosphine dichloride and 1,1,3,3-tetramethyl-1,3-disiloxanediol were mixed uniformly in a molar ratio of 0.5:0.5:1, activated silver-loaded silica in an amount of 0.35 times the mass of spirocyclic phosphate diacyl chloride was added, stirred at 25°C and 250 r / min for 70 min, heated to 85°C at a heating rate of 1°C / min and continued to stir for 3.5 h, centrifuged and washed 4 times with anhydrous ethanol to obtain modified silver-loaded silica;

[0036] (4) Weigh 95 parts of F401 polypropylene, 0.35 parts of diisopropylbenzene peroxide, and 4.5 parts of modified silver-loaded silica according to their mass fractions; add each component into an internal mixer, mix at 185°C, 65 r / min for 11 min, hot press at 185°C, 13 MPa for 18 min, cool naturally to 100°C and keep warm for 7 h, and take out after cooling to room temperature to obtain a fire-retardant polymer material.

[0037] Example 3

[0038] A method for preparing a fire-retardant polymer material, the method for preparing a fire-retardant polymer material mainly comprises the following preparation steps:

[0039] (1) Ethyl orthosilicate and anhydrous ethanol are mixed in a mass ratio of 1:10 to prepare an ethyl orthosilicate solution; 1 mol / L ammonia water, hexadecyltrimethylammonium bromide and 20-30% ethanol aqueous solution are mixed in a mass ratio of 1:1:55, stirred at 30°C and 1000 r / min for 30 min, stirred continuously and added with the ethyl orthosilicate solution, the ratio of the molar amount of ethyl orthosilicate to the molar amount of hexadecyltrimethylammonium bromide in the ethyl orthosilicate solution is 4:1, stirred continuously at 30°C for 8 h, stopped stirring and allowed to stand for 8 h, centrifuged and washed with pure water 5 times, dried at 70°C for 4 h, and porous silica was obtained;

[0040] (2) 1 mol / L hydrochloric acid aqueous solution and anhydrous ethanol were mixed in a volume ratio of 1:2 to prepare an extracting solution; the porous silica was immersed in the extracting solution, stirred at 65°C and 300 r / min for 8 h, centrifuged and washed with pure water for 3 times, and dried at 70°C for 3 h to obtain the porous silica with the template removed; the porous silica with the template removed was placed in a container, the pressure was adjusted to 50 Pa with a vacuum pump, 0.2 mol / L silver nitrate solution was added to immerse the porous silica with the template removed, ultrasonically dispersed for 10 min, restored to normal pressure and allowed to stand for 30 min, centrifuged and placed in a container, and hydrogen chloride gas was introduced at a rate of 1 mL / s for 40 min, then washed with pure water for 3 times and filtered, and dried at 70°C for 3 h to obtain silver-loaded silica;

[0041] (3) Silver-loaded silica, pure water and anhydrous ethanol were mixed uniformly in a mass ratio of 1:3:10, stirred at 30°C and 800 r / min for 20 min, then 0.4 times the mass of the silver-loaded silica in a 1 mol / L sodium hydroxide solution and 3 times the mass of the silver-loaded silica in an ethyl orthosilicate solution were added, ultrasonicated at 30°C for 1 h, centrifuged and washed with anhydrous ethanol for 5 times, and dried at 70°C for 6 h to obtain activated silver-loaded silica; spirocyclic phosphate dihydrate was added to the mixture, and the mixture was stirred for 20 min at 800 r / min for 20 min. Acyl chloride, allylphosphine dichloride and 1,1,3,3-tetramethyl-1,3-disiloxanediol were uniformly mixed in a molar ratio of 0.5:0.5:1, activated silver-loaded silica in an amount of 0.4 times the mass of spirocyclic phosphate diacyl chloride was added, stirred at 30°C and 300 r / min for 60 min, heated to 85°C at a heating rate of 1°C / min and continued to stir for 4 h, centrifuged and washed with anhydrous ethanol for 5 times to obtain modified silver-loaded silica;

[0042] (4) Weigh 100 parts of F401 polypropylene, 0.4 parts of diisopropylbenzene peroxide, and 5 parts of modified silver-loaded silica according to their mass fractions; add each component into an internal mixer, mix at 190°C, 70 r / min for 10 min, hot press at 190°C, 15 MPa for 15 min, cool naturally to 100°C and keep warm for 6 h, and take out after cooling to room temperature to obtain a fire-retardant polymer material.

[0043] Comparative Example 1

[0044] The difference between Comparative Example 1 and Example 2 is only step (2), and step (2) is modified as follows: placing the porous silica at 550° C. for 6 h to obtain the porous silica with the template removed; placing the porous silica with the template removed in a container, adjusting the pressure to 50 Pa with a vacuum pump, adding 0.2 mol / L silver nitrate solution to immerse the porous silica with the template removed, ultrasonically dispersing for 10 min, restoring normal pressure and standing for 30 min, centrifuging and placing in a container, and passing hydrogen chloride gas at a rate of 1 mL / s for 35 min, then washing with pure water 4 times and filtering, and drying at 70° C. for 3 h to obtain silver-loaded silica.

[0045] Comparative Example 2

[0046] The difference between Comparative Example 2 and Example 2 is only in step (2), and step (2) is modified as follows: immersing the porous silica in the extract, stirring at 62°C and 250 r / min for 9 h, centrifuging and washing with pure water for 3 times, and drying at 70°C for 3 h to obtain the porous silica with the template removed; placing the porous silica with the template removed in a container, adding 0.2 mol / L silver nitrate solution at normal pressure to immerse the porous silica with the template removed, ultrasonically dispersing for 10 min, standing for 30 min, centrifuging and placing in a container, and passing hydrogen chloride gas at a rate of 1 mL / s for 35 min, then washing with pure water for 4 times and filtering, and drying at 70°C for 3 h to obtain silver-loaded silica.

[0047] Comparative Example 3

[0048] The difference between Comparative Example 3 and Example 2 is only in step (2), and step (2) is modified as follows: placing the porous silica at 550° C. for 6 h to obtain the porous silica with the template removed; placing the porous silica with the template removed in a container, adding 0.2 mol / L silver nitrate solution at normal pressure to immerse the porous silica with the template removed, ultrasonically dispersing for 10 min, standing for 30 min, centrifuging and placing in a container, and passing hydrogen chloride gas at a rate of 1 mL / s for 35 min, then washing with pure water 4 times and filtering, and drying at 70° C. for 3 h to obtain silver-loaded silica.

[0049] Comparative Example 4

[0050] The difference between Comparative Example 4 and Example 2 is only in step (3). Step (3) is modified as follows: spirocyclic phosphate dichloride, allyl phosphine dichloride and 1,1,3,3-tetramethyl-1,3-disiloxane diol are uniformly mixed in a molar ratio of 0.5:0.5:1, 0.4 times the mass of spirocyclic phosphate dichloride is added with silver-loaded silica, the mixture is stirred at 30°C and 300 r / min for 60 min, the temperature is increased to 85°C at a heating rate of 1°C / min and the stirring reaction is continued for 4 h, the mixture is centrifuged and washed with anhydrous ethanol 5 times to obtain modified silver-loaded silica.

[0051] Comparative Example 5

[0052] The difference between Comparative Example 5 and Example 2 is only in step (3), and step (3) is modified as follows: silver-loaded silica, pure water and anhydrous ethanol are uniformly mixed in a mass ratio of 1:2.5:9, stirred at 25°C and 700 r / min for 22 min, then 0.35 times the mass of the silver-loaded silica in a 1 mol / L sodium hydroxide solution and 2.5 times the mass of the silver-loaded silica in an ethyl orthosilicate solution are added, ultrasonicated at 25°C for 1.5 h, centrifuged and washed with anhydrous ethanol 4 times, and dried at 65°C for 7 min. h to obtain activated silver-loaded silica; spirocyclic phosphate dichloride and 1,1,3,3-tetramethyl-1,3-disiloxane diol were uniformly mixed in a molar ratio of 1:1, and 0.35 times the mass of spirocyclic phosphate dichloride activated silver-loaded silica was added, and the mixture was stirred at 25°C and 250 r / min for 70 min, and the temperature was increased to 85°C at a heating rate of 1°C / min and the stirring reaction was continued for 3.5 h, and the mixture was centrifuged and washed 4 times with anhydrous ethanol to obtain modified silver-loaded silica.

[0053] Comparative Example 6

[0054] A method for preparing a fire-retardant polymer material, the method for preparing a fire-retardant polymer material mainly comprises the following preparation steps:

[0055] (1) Ethyl orthosilicate and anhydrous ethanol are mixed in a mass ratio of 1:9 to prepare an ethyl orthosilicate solution; 1 mol / L ammonia water, hexadecyltrimethylammonium bromide and a 25% ethanol aqueous solution are mixed in a mass ratio of 1:1:50, stirred at 25°C and 900 r / min for 35 minutes, stirred continuously and added with the ethyl orthosilicate solution, the ratio of the molar amount of ethyl orthosilicate to the molar amount of hexadecyltrimethylammonium bromide in the ethyl orthosilicate solution is 4:1, stirred continuously at 28°C for 9 hours, stopped stirring and allowed to stand for 10 hours, centrifuged and washed with pure water 4 times, dried at 70°C for 3.5 hours, and porous silica is obtained;

[0056] (2) 1 mol / L hydrochloric acid aqueous solution and anhydrous ethanol were mixed in a volume ratio of 1:2 to prepare an extracting solution; the porous silica was immersed in the extracting solution, stirred at 62°C and 250 r / min for 9 h, centrifuged and washed with pure water for 3 times, and dried at 70°C for 3 h to obtain the porous silica with the template removed; the porous silica with the template removed was placed in a container, the pressure was adjusted to 50 Pa with a vacuum pump, 0.2 mol / L silver nitrate solution was added to immerse the porous silica with the template removed, ultrasonically dispersed for 10 min, restored to normal pressure and allowed to stand for 30 min, centrifuged and placed in a container, and hydrogen chloride gas was introduced at a rate of 1 mL / s for 35 min, then washed with pure water 4 times and filtered, and dried at 70°C for 3 h to obtain silver-loaded silica;

[0057] (3) Weigh 95 parts of F401 polypropylene, 0.35 parts of diisopropylbenzene peroxide, and 4.5 parts of silver-loaded silica according to their mass fractions; add each component into an internal mixer, mix at 185°C, 65 r / min for 11 min, hot press at 185°C, 13 MPa for 18 min, cool naturally to 100°C and keep warm for 7 h, and take out after cooling to room temperature to obtain a fire-retardant polymer material.

[0058] Test Example 1

[0059] Tensile strength test

[0060] Tensile strength test method: The materials of each embodiment and comparative example were made into specimens with a size of 50 mm in length, 4 mm in width and 0.12 mm in thickness, and tested using an INSTRON 1121 material testing machine with a tensile force of 1000 N and a tensile speed of 50 mm / min. The test standard was GB / T1040.1. The results are shown in Table 1.

[0061]

[0062] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 6 in Table 1, it can be found that the fire-retardant polymer material prepared by the present invention has good tensile strength.

[0063] Examples 1 to 3 and Comparative Example 4 illustrate that activation treatment of silver-loaded silica can make the surface have higher reactivity, improve the degree of modification, and thus improve the tensile strength.

[0064] By comparing the data of Examples 1 to 3 and Comparative Examples 5 and 6, it can be found that the tensile strength of Examples 1 to 3 is high, which indicates that after modification, the dispersibility of silver-loaded silica is improved, and the double bonds introduced into allyl phosphine dichloride can be subsequently initiated by diisopropylbenzene peroxide and cross-linked with polypropylene to form a cross-linked network structure, thereby improving the tensile strength.

[0065] Test Example 2

[0066] Antimicrobial performance testing

[0067] Antibacterial performance test method: Escherichia coli was activated to obtain a concentration of 10 7 Then, 0.1 g of each film was weighed and immersed in 10 mL of 100-fold diluted bacterial suspension (10 5 CFU / mL), and the bacterial suspension with pure linear low-density polyethylene film was placed at room temperature for 48 hours as a blank group. Finally, the bacterial suspension of each group was diluted 100 times, and 100 μL was evenly applied on the surface of TSA culture medium. After culturing at 37°C for 24 hours, the bacterial colony growth was counted and the inhibition rate was calculated. Inhibition rate = (AB) / A, where A is the bacterial count of pure LDPE film and B is the bacterial count of the sample. The results are shown in Table 2.

[0068]

[0069] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 6 in Table 2, it can be found that the fire-retardant polymer material prepared by the present invention has good antibacterial properties.

[0070] By comparing the data of Examples 1 to 3 and Comparative Examples 1 to 3, it can be found that the antibacterial rates of Examples 1 to 3 are high, which shows that the method of removing the template agent adopts the extraction method, which will not cause the collapse or blockage of the pores compared to burning, and can better load silver ions. The immersion method can make the silver nitrate solution enter the pores through vacuuming, and better load, thereby improving the subsequent sterilization effect.

[0071] Test Example 3

[0072] Flame retardant performance test

[0073] Flame retardant performance test method: Test the limiting oxygen index according to GB / T 2406 standard. The results are shown in Table 3.

[0074]

[0075] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 6 in Table 3, it can be found that the fire-retardant polymer material prepared by the present invention has good flame retardant properties.

[0076] By comparing the data of Examples 1 to 3 and Comparative Example 4, it can be found that the limiting oxygen index of Examples 1 to 3 is high, which indicates that the activation treatment of the silver-loaded silica makes the surface have higher reactivity, improves the degree of modification, and thus improves the flame retardant performance.

[0077] By comparing the data of Examples 1 to 3 and Comparative Example 6, it can be found that the limiting oxygen index of Examples 1 to 3 is high, which indicates that after modification, long silicon-phosphorus chains are generated on the surface of the silver-loaded silica, which improves the dispersibility, and the silicon-phosphorus elements coordinate the flame retardancy and have a good flame retardant effect.

[0078] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a fire-retardant polymer material, characterized in that: The method comprises the following preparation steps: (1) 1 mol / L ammonia water, hexadecyltrimethylammonium bromide and 20-30% ethanol aqueous solution are mixed in a mass ratio of 1:1:(45-55), stirred at 20-30°C and 800-1000 r / min for 30-40 min, and then added with tetraethyl orthosilicate solution. The ratio of the molar amount of tetraethyl orthosilicate to the molar amount of hexadecyltrimethylammonium bromide in the tetraethyl orthosilicate solution is 4:

1. The reaction is continued with stirring at 25-30°C for 8-10 h, and then the stirring is stopped and the mixture is allowed to stand for 8-12 h. The mixture is centrifuged and washed with pure water for 3-5 times, and then dried at 70°C for 3-4 h to obtain porous silica. (2) 1 mol / L hydrochloric acid aqueous solution and anhydrous ethanol were mixed in a volume ratio of 1:2 to prepare an extracting solution; the porous silica was immersed in the extracting solution, stirred at 60-65°C and 200-300 r / min for 8-10 h, centrifuged and washed with pure water for 3 times, and dried at 70°C for 3 h to obtain the porous silica with the template removed; the porous silica with the template removed was placed in a container, the pressure was adjusted to 50 Pa with a vacuum pump, 0.2 mol / L silver nitrate solution was added to immerse the porous silica with the template removed, ultrasonically dispersed for 10 min, restored to normal pressure and allowed to stand for 30 min, centrifuged and placed in a container, and hydrogen chloride gas was introduced at a rate of 1 mL / s for 30-40 min, then washed with pure water for 3-5 times and filtered, and dried at 70°C for 3 h to obtain silver-loaded silica; (3) Mix silver-loaded silica, pure water and anhydrous ethanol in a mass ratio of 1:(2-3):(8-10), stir at 20-30°C and 600-800 r / min for 20-25 min, then add 0.3-0.4 times the mass of the silver-loaded silica in a 1 mol / L sodium hydroxide solution and 2-3 times the mass of the silver-loaded silica in an ethyl orthosilicate solution, ultrasonicate at 20-30°C for 1-2 h, centrifuge and wash with anhydrous ethanol for 3-5 times, and dry at 60-70°C for 6-8 h to obtain activated silver-loaded silica.

1. Mix spirocyclic phosphate dichloride, allyl phosphine dichloride and 1,1,3,3-tetramethyl-1,3-disiloxane diol in a molar ratio of 0.5:0.5:1, add activated silver-loaded silica in an amount of 0.3-0.4 times the mass of spirocyclic phosphate dichloride, stir and react at 200-300 r / min for 60-80 min at 20-30° C., heat to 85° C. at a heating rate of 1° C. / min and continue stirring and reacting for 3-4 h, centrifuge and wash with anhydrous ethanol for 3-5 times to obtain modified silver-loaded silica; (4) Weigh 90-100 parts of polypropylene, 0.3-0.4 parts of diisopropylbenzene peroxide, and 4-5 parts of modified silver-loaded silica according to their mass fractions; add the components into an internal mixer, mix at 180-190°C and 60-70 r / min for 10-12 min, hot press at 180-190°C and 12-15 MPa for 15-20 min, cool naturally to 100°C and keep warm for 6-8 h, and take out after cooling to room temperature to obtain a fire-retardant polymer material.

2. The method for preparing a fire-retardant polymer material according to claim 1, characterized in that: The tetraethyl orthosilicate solution in step (1) is prepared by uniformly mixing tetraethyl orthosilicate and anhydrous ethanol in a mass ratio of 1:(8-10).

3. The method for preparing a fire-retardant polymer material according to claim 1, characterized in that: The model of the polypropylene in step (3) is F401.

4. A fire-retardant polymer material prepared according to the method for preparing a fire-retardant polymer material according to any one of claims 1 to 3.