Glass fiber reinforced plastic based on vinyl ester resin and preparation method thereof

By introducing high-temperature-resistant modified vinyl ester resin and modified glass fiber into glass fiber reinforced vinyl ester resin, the problem of poor performance of existing materials in high temperatures and fires is solved, and the excellent mechanical properties and resistance of the materials are achieved Fuel performance, suitable for high performance requirements.

CN118325295BActive Publication Date: 2024-11-05MILIKUDO GLASS FIBER REINFORCED PLASTIC TAIZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410617559.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-11-05
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

There is room for improvement in strength, heat resistance and flame retardancy of glass fiber reinforced vinyl ester resin plastics on the market, resulting in poor performance in high temperature environments and fires, limiting their high requirements for flame retardant and mechanical properties. application in the field.

Method used

Using high-temperature-resistant modified vinyl ester resin and modified glass fiber, glass fiber reinforced plastics with excellent mechanical properties, high-temperature resistance and flame retardant properties are prepared through specific synthesis steps and processes. The method includes introducing organic phosphorus and organic nitrogen into the reaction of materials such as melamine, 3,5-dimethoxybenzaldehyde, forming a ring structure, improving the crosslinking degree and curing speed of the material, and treating it with a silane coupling agent Modify glass fibers to improve dispersion and bonding.

Benefits of technology

The prepared glass fiber reinforced plastic has excellent mechanical properties, high temperature resistance and flame retardant properties. It can be used stably in a high-temperature environment for a long time, reduces fire risks, and is simple and easy to industrially produce.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of plastics, and in particular to glass fiber reinforced plastics based on vinyl ester resins and a preparation method thereof, and is used to solve the problem that the glass fiber reinforced vinyl ester resin plastics currently on the market still have room for improvement in terms of strength, heat resistance and flame retardancy, resulting in poor performance in high temperature environments and fires. In the preparation method, the glass fiber reinforced plastics are prepared using high temperature resistant modified vinyl ester resins and modified glass fibers as main raw materials, so that the prepared glass fiber reinforced plastics have the following advantages: excellent high temperature resistance and long-term stable use in high temperature environments; good flame retardancy and the ability to effectively reduce fire risks; excellent mechanical properties and high strength; simple preparation process and easy industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of plastics, in particular to glass fiber reinforced plastics based on vinyl ester resin and a preparation method thereof. Background Art

[0002] Vinyl ester resin is obtained by addition reaction of epoxy resin and unsaturated monocarboxylic acid containing double bonds. It not only retains the basic chain segment of epoxy resin, but also has excellent corrosion resistance and mechanical properties, and is connected with unsaturated double bonds, which has good processing properties. Therefore, vinyl ester resin is widely used in chemical industry, metallurgy, construction and other fields. Glass fiber, as a lightweight and high-strength reinforcing material, can be combined with vinyl ester resin to prepare composite materials with excellent performance. With the advancement of science and technology and the development of industry, the performance requirements of polymer materials are getting higher and higher. However, the glass fiber reinforced vinyl ester resin plastics on the market still have room for improvement in strength, heat resistance and flame retardancy, resulting in poor performance in high temperature environment and fire, which seriously limits its application in fields with high requirements for flame retardancy and mechanical properties. Therefore, it is of great practical significance to develop a glass fiber reinforced plastic based on vinyl ester resin with excellent mechanical properties, high temperature resistance and flame retardancy and a preparation method. Summary of the invention

[0003] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a glass fiber reinforced plastic based on vinyl ester resin and a preparation method, which solves the problem that the glass fiber reinforced vinyl ester resin plastics currently on the market still have room for improvement in strength, heat resistance and flame retardancy, resulting in poor performance in high temperature environments and fires.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] Glass fiber reinforced plastic based on vinyl ester resin, comprising the following components in parts by weight:

[0006] 80-120 parts of high temperature resistant modified vinyl ester resin, 6-24 parts of modified glass fiber, 35-55 parts of diluent, 1.3-1.9 parts of accelerator and 0.9-1.5 parts of initiator;

[0007] Wherein, the high temperature resistant modified vinyl ester resin is prepared by the following steps:

[0008] Step A1: adding melamine, 3,5-dimethoxybenzaldehyde and anhydrous ethanol to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stirring the mixture for 20-30 min at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heating the mixture to reflux and continuing the stirring reaction for 8-10 h. After the reaction is completed, the reaction product is cooled to room temperature, then vacuum filtered, and the filter cake is washed with distilled water for 3-5 times, then placed in a vacuum drying oven, and dried at a temperature of 80-85° C. for 3-5 h to obtain an intermediate 1;

[0009] Step A2: Add intermediate 1, DOPO and N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas pipe and a reflux condenser, introduce nitrogen protection, stir and react for 5-10 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heat to reflux and continue stirring and reacting for 8-10 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain intermediate 2;

[0010] Step A3: Add intermediate 2 and dichloromethane to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas pipe and a constant pressure dropping funnel, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of -5-0°C and a stirring rate of 300-400r / min, then add boron tribromide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, the temperature is raised to 25-30°C and the stirring reaction is continued for 10-15 hours. After the reaction is completed, the reaction product is added to ice water, and then vacuum filtered. The filter cake is placed in a vacuum drying oven and dried at a temperature of 60-65°C for 3-5 hours to obtain intermediate 3;

[0011] Step A4: Add intermediate 3, epichlorohydrin and benzyltriethylammonium chloride to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir and react for 6-8 hours at a temperature of 90-95° C. and a stirring rate of 300-400 r / min, then add sodium hydroxide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, continue to stir and react for 3-5 hours. After the reaction is completed, cool the reaction product to room temperature, and then remove the solvent by rotary evaporation to obtain intermediate 4;

[0012] Step A5: Add intermediate 4 and hydroquinone to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir and react for 10-15 minutes at a temperature of 50-55°C and a stirring rate of 300-400r / min, then add benzyltriethylammonium chloride and continue to stir and react for 5-10 minutes, then add acrylic acid dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, the temperature is raised to 100-110°C and the stirring reaction is continued for 2-3 hours. After the reaction is completed, the reaction product is cooled to room temperature to obtain a high temperature resistant modified vinyl ester resin.

[0013] As a further solution of the present invention: the usage ratio of the melamine, 3,5-dimethoxybenzaldehyde and anhydrous ethanol in step A1 is 10 mmol: 33-37 mmol: 50-60 mL.

[0014] As a further scheme of the present invention: the usage ratio of the intermediate 1, DOPO and N,N-dimethylformamide in step A2 is 10 mmol: 30-35 mmol: 90-100 mL.

[0015] As a further solution of the present invention: the usage ratio of the intermediate 2, dichloromethane and boron tribromide solution in step A3 is 10 mmol: 100-120 mL: 50-55 mL.

[0016] As a further solution of the present invention: the boron tribromide solution in step A3 is a solution formed by dissolving boron tribromide in dichloromethane at a ratio of 8-10 mmol:5 mL.

[0017] As a further scheme of the present invention: the usage ratio of the intermediate 3, epichlorohydrin, benzyltriethylammonium chloride and sodium hydroxide solution in step A4 is 10 mmol: 40-50 mL: 2.5-3.5 g: 60-80 mL.

[0018] As a further solution of the present invention: the mass fraction of the sodium hydroxide solution in step A4 is 20-25%.

[0019] As a further solution of the present invention: the usage ratio of the intermediate 4, hydroquinone, benzyltriethylammonium chloride and acrylic acid in step A5 is 100g: 0.05-0.1g: 0.3-0.9g: 40-70g.

[0020] As a further solution of the present invention: the modified glass fiber is prepared by the following steps:

[0021] Step B1: adding glass fiber and anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, introducing nitrogen protection, stirring the reaction for 5-10 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heating to reflux and continuing to stir the reaction for 6-8 hours, cooling the reaction product to room temperature after the reaction is completed, and then vacuum filtering, washing the filter cake with distilled water for 3-5 times, and then placing it in a vacuum drying oven, and drying it at a temperature of 60-65° C. for 2-3 hours to obtain washed glass fiber;

[0022] Step B2: Add washed glass fiber, hexadecyltrimethylammonium bromide, deionized water and anhydrous ethanol to a three-necked flask equipped with a thermometer, a stirrer and a reflux condenser, stir and react for 10-15 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add silane coupling agent KH-570 and continue stirring and reacting for 8-10 hours under the condition of heating to reflux. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed with distilled water for 3-5 times, and then placed in a vacuum drying oven and dried at a temperature of 60-65°C for 2-3 hours to obtain modified glass fiber.

[0023] As a further solution of the present invention: the usage ratio of the glass fiber and anhydrous acetone in step B1 is 2g:20-25mL.

[0024] As a further solution of the present invention: the glass fiber in step B1 is an alkali-free glass fiber with a length of 3 mm and a diameter of 20 μm.

[0025] As a further solution of the present invention: the usage ratio of the washed glass fiber, hexadecyltrimethylammonium bromide, deionized water, anhydrous ethanol and silane coupling agent KH-570 in step B2 is 10g: 0.05-0.09g: 25-35mL: 100-110mL: 7.5-15g.

[0026] As a further solution of the present invention: a method for preparing glass fiber reinforced plastic based on vinyl ester resin comprises the following steps:

[0027] Step 1: Weigh 80-120 parts of high temperature resistant modified vinyl ester resin, 6-24 parts of modified glass fiber, 35-55 parts of diluent, 1.3-1.9 parts of accelerator and 0.9-1.5 parts of initiator according to weight parts, and set aside;

[0028] Step 2: Add the high temperature resistant modified vinyl ester resin, modified glass fiber and diluent into a mixer, stir and mix for 30-50 minutes at a temperature of 45-50°C and a stirring rate of 300-400r / min, then add the accelerator and initiator and continue to stir and mix for 5-8 minutes, then pour into a mold, and then place in an oven, and cure at a temperature of 70-75°C for 2-2.5 hours, and then heat to 95-100°C and cure for 0.5-1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0029] As a further solution of the present invention: the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate.

[0030] Beneficial effects of the present invention:

[0031] The glass fiber reinforced plastic based on vinyl ester resin and the preparation method of the present invention are as follows: a high temperature resistant modified vinyl ester resin, modified glass fiber and a diluent are added to a mixer and stirred and mixed, a accelerator and an initiator are added and stirred and mixed continuously, the mixture is poured into a mold, and the mixture is placed in an oven for curing to obtain the glass fiber reinforced plastic based on vinyl ester resin; in the preparation method, the high temperature resistant modified vinyl ester resin and the modified glass fiber are used as main raw materials to prepare the glass fiber reinforced plastic, so that the prepared glass fiber reinforced plastic has the following advantages: excellent high temperature resistance and can be used stably for a long time in a high temperature environment; good flame retardant performance and can effectively reduce the risk of fire; excellent mechanical properties and high strength; simple preparation process and easy to realize industrial production;

[0032] In the process of preparing glass fiber reinforced plastics based on vinyl ester resin, a high temperature resistant modified vinyl ester resin is first prepared. First, melamine and 3,5-dimethoxybenzaldehyde are reacted, and the amino group on melamine and the aldehyde group on 3,5-dimethoxybenzaldehyde form a Schiff base structure to obtain intermediate 1. Then, intermediate 1 and DOPO are reacted, and the C=N on intermediate 1 reacts with the PH on DOPO to introduce organic phosphorus to obtain intermediate 2. Then, under the action of boron tribromide, the methoxy group on intermediate 2 is converted into hydroxyl group to obtain intermediate 3. Then, intermediate 3 and epichlorohydrin are reacted, and the hydroxyl group on intermediate 3 first causes epichlorohydrin to undergo a ring-opening reaction, and then a ring-closing reaction occurs under the condition of sodium hydroxide solution to introduce Epoxy groups are formed to obtain intermediate 4, and then the epoxy groups on intermediate 4 react with the carboxyl groups on acrylic acid to obtain a high-temperature resistant modified vinyl ester resin; the molecular structure of the high-temperature resistant modified vinyl ester resin contains a large number of cyclic structures, which give it excellent mechanical properties and high-temperature stability, and the introduction of organic nitrogen and organic phosphorus can greatly improve its high-temperature resistance and flame retardant properties, and the molecular structure of the high-temperature resistant modified vinyl ester resin has a large number of alkenyl groups, so that it has a high degree of cross-linking during the curing process, and the mechanical properties are further improved, and it has a fast curing speed, a low curing temperature, and excellent material properties; therefore, the glass fiber reinforced plastic with the high-temperature resistant modified vinyl ester resin as the main raw material has excellent mechanical properties, high-temperature resistance and flame retardant properties;

[0033] In the process of preparing glass fiber reinforced plastics based on vinyl ester resin, a modified glass fiber is also prepared. First, the glass fiber is treated with anhydrous acetone to fully remove impurities on the surface of the glass fiber to obtain washed glass fiber. Then, the washed glass fiber is treated with a silane coupling agent KH-570. The siloxane on the silane coupling agent KH-570 is hydrolyzed to form silanol, which is then dehydrated, condensed and grafted onto the glass fiber to obtain a modified glass fiber. After modification, the modified glass fiber is endowed with excellent dispersibility, so that it can be evenly dispersed in the plastic matrix, effectively improving the performance of the plastic matrix, and the introduced olefin group can react with the olefin group in the plastic matrix during the curing process, and connect to the plastic matrix in the form of a chemical bond, further enhancing the bonding force between the two, and further improving the mechanical properties. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Embodiment 1:

[0036] This embodiment is a method for preparing glass fiber reinforced plastic based on vinyl ester resin, comprising the following steps:

[0037] Step S1: 10 mmol of melamine, 33 mmol of 3,5-dimethoxybenzaldehyde and 50 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was stirred for reaction at 25° C. and a stirring rate of 300 r / min for 20 min, and then the mixture was heated to reflux and continued to stir for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed with distilled water for 3 times, and then placed in a vacuum drying oven and dried at 80° C. for 3 h to obtain an intermediate 1;

[0038] Step S2: 10 mmol of intermediate 1, 30 mmol of DOPO and 90 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas pipe and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 300 r / min for 5 min, and then the temperature was raised to reflux and the stirring reaction was continued for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;

[0039] Step S3: 10 mmol of intermediate 2 and 100 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a constant pressure dropping funnel, and nitrogen protection was introduced. The mixture was stirred for 20 min at a temperature of -5°C and a stirring rate of 300 r / min. Then, 50 mL of a boron tribromide solution formed by dissolving 8 mmol:5 mL of boron tribromide in dichloromethane was added dropwise while stirring. The dropping rate was controlled to be 1 drop / s. After the addition was completed, the mixture was heated to 25°C and continued to stir for 10 h. After the reaction was completed, the reaction product was added to ice water, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at 60°C for 3 h to obtain intermediate 3;

[0040] Step S4: 10 mmol of intermediate 3, 40 mL of epichlorohydrin and 2.5 g of benzyltriethylammonium chloride were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture was stirred for reaction at a temperature of 90° C. and a stirring rate of 300 r / min for 6 h, and then 60 mL of a 20% sodium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 4;

[0041] Step S5: 100 g of intermediate 4 and 0.05 g of hydroquinone are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred at 50° C. and a stirring rate of 300 r / min for 10 min, and then 0.3 g of benzyltriethylammonium chloride is added and the stirring reaction is continued for 5 min, and then 40 g of acrylic acid is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the addition is completed, the mixture is heated to 100° C. and the stirring reaction is continued for 2 h. After the reaction is completed, the reaction product is cooled to room temperature to obtain a high temperature resistant modified vinyl ester resin;

[0042] Step S6: adding 2 g of alkali-free glass fiber with a length of 3 mm and a diameter of 20 μm and 20 mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, introducing nitrogen protection, stirring the reaction for 5 min at a temperature of 25° C. and a stirring rate of 300 r / min, then heating to reflux and continuing to stir the reaction for 6 h, cooling the reaction product to room temperature after the reaction is completed, and then vacuum filtering, washing the filter cake with distilled water 3 times, and then placing it in a vacuum drying oven, and drying it at a temperature of 60° C. for 2 h to obtain washed glass fiber;

[0043] Step S7: 10 g of washed glass fiber, 0.05 g of hexadecyltrimethylammonium bromide, 25 mL of deionized water and 100 mL of anhydrous ethanol were added to a three-necked flask equipped with a thermometer, a stirrer and a reflux condenser, and stirred for reaction at a temperature of 25 ° C. and a stirring rate of 300 r / min for 10 min, then 7.5 g of silane coupling agent KH-570 was added and the temperature was raised to reflux and the stirring reaction was continued for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filter cake was washed with distilled water 3 times, and then placed in a vacuum drying oven and dried at a temperature of 60 ° C. for 2 h to obtain modified glass fiber;

[0044] Step S8: weighing 80 parts of high temperature resistant modified vinyl ester resin, 6 parts of modified glass fiber, 35 parts of diluent, 1.3 parts of accelerator and 0.9 parts of initiator according to weight parts for standby use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate;

[0045] Step S9: Add the high temperature resistant modified vinyl ester resin, modified glass fiber and diluent into a mixer, stir and mix for 30 minutes at a temperature of 45°C and a stirring rate of 300 r / min, then add the accelerator and initiator and continue to stir and mix for 5 minutes, then pour into a mold, and then place in an oven, cure at a temperature of 70°C for 2 hours, and then heat to 95°C and cure for 0.5 hours to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0046] Embodiment 2:

[0047] This embodiment is a method for preparing glass fiber reinforced plastic based on vinyl ester resin, comprising the following steps:

[0048] Step S1: 10 mmol of melamine, 35 mmol of 3,5-dimethoxybenzaldehyde and 55 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 25 min, then the temperature was raised to reflux and the stirring reaction was continued for 9 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed with distilled water for 4 times, and then placed in a vacuum drying oven and dried at a temperature of 82° C. for 4 h to obtain intermediate 1;

[0049] Step S2: 10 mmol of intermediate 1, 32 mmol of DOPO and 95 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 28° C. and a stirring rate of 350 r / min for 8 min, and then the temperature was raised to reflux and the stirring reaction was continued for 9 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;

[0050] Step S3: 10 mmol of intermediate 2 and 110 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a constant pressure dropping funnel, and nitrogen protection was introduced. The mixture was stirred for 25 min at a temperature of -3°C and a stirring rate of 350 r / min. Then, 52 mL of a boron tribromide solution formed by dissolving boron tribromide in dichloromethane at a ratio of 9 mmol:5 mL was added dropwise while stirring. The dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to 28°C and the stirring reaction was continued for 12 h. After the reaction was completed, the reaction product was added to ice water, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 62°C for 4 h to obtain intermediate 3;

[0051] Step S4: 10 mmol of intermediate 3, 45 mL of epichlorohydrin and 3 g of benzyltriethylammonium chloride were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred for reaction at a temperature of 92° C. and a stirring rate of 350 r / min for 7 h, and then 70 mL of a 22% sodium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 4;

[0052] Step S5: 100 g of intermediate 4 and 0.08 g of hydroquinone were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture was stirred for reaction at a temperature of 52° C. and a stirring rate of 350 r / min for 12 min, and then 0.6 g of benzyltriethylammonium chloride was added and the mixture was stirred for reaction for 8 min, and then 55 g of acrylic acid was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the mixture was heated to 105° C. and the mixture was stirred for reaction for 2.5 h. After the reaction was completed, the reaction product was cooled to room temperature to obtain a high temperature resistant modified vinyl ester resin;

[0053] Step S6: adding 2 g of alkali-free glass fiber with a length of 3 mm and a diameter of 20 μm and 22 mL of anhydrous acetone into a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, introducing nitrogen protection, stirring the reaction for 8 min at a temperature of 28° C. and a stirring rate of 350 r / min, then heating to reflux and continuing to stir the reaction for 7 h, cooling the reaction product to room temperature after the reaction is completed, and then vacuum filtering, washing the filter cake with distilled water 4 times, and then placing it in a vacuum drying oven, and drying it at a temperature of 62° C. for 2.5 h to obtain washed glass fiber;

[0054] Step S7: 10 g of washed glass fiber, 0.07 g of hexadecyltrimethylammonium bromide, 30 mL of deionized water and 105 mL of anhydrous ethanol were added to a three-necked flask equipped with a thermometer, a stirrer and a reflux condenser, and stirred for reaction at a temperature of 28 ° C. and a stirring rate of 350 r / min for 12 min, then 11 g of silane coupling agent KH-570 was added and the temperature was raised to reflux and the stirring reaction was continued for 9 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filter cake was washed with distilled water 4 times, and then placed in a vacuum drying oven and dried at a temperature of 62 ° C. for 2.5 h to obtain modified glass fiber;

[0055] Step S8: weighing 100 parts of high temperature resistant modified vinyl ester resin, 15 parts of modified glass fiber, 45 parts of diluent, 1.6 parts of accelerator and 1.2 parts of initiator according to weight parts for later use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate;

[0056] Step S9: Add the high temperature resistant modified vinyl ester resin, modified glass fiber and diluent into a mixer, stir and mix for 40 minutes at a temperature of 48°C and a stirring rate of 350r / min, then add the accelerator and initiator and continue to stir and mix for 7 minutes, then pour into a mold, and then place in an oven, cure at a temperature of 72°C for 2 hours, and then heat to 98°C and cure for 1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0057] Embodiment 3:

[0058] This embodiment is a method for preparing glass fiber reinforced plastic based on vinyl ester resin, comprising the following steps:

[0059] Step S1: 10 mmol of melamine, 37 mmol of 3,5-dimethoxybenzaldehyde and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min, and then the mixture was heated to reflux and continued to be stirred for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed with distilled water for 5 times, and then placed in a vacuum drying oven and dried at a temperature of 85° C. for 5 h to obtain an intermediate 1;

[0060] Step S2: 10 mmol of intermediate 1, 35 mmol of DOPO and 100 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, and nitrogen protection was introduced. The mixture was stirred at 30° C. and a stirring rate of 400 r / min for 10 min, and then the temperature was raised to reflux and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;

[0061] Step S3: 10 mmol of intermediate 2 and 120 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a constant pressure dropping funnel, and nitrogen protection was introduced. The mixture was stirred for 30 min at a temperature of 0°C and a stirring rate of 400 r / min. Then, 55 mL of a boron tribromide solution formed by dissolving boron tribromide in dichloromethane at a ratio of 10 mmol:5 mL was added dropwise while stirring. The dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 30°C and the stirring reaction was continued for 15 h. After the reaction was completed, the reaction product was added to ice water, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 65°C for 5 h to obtain intermediate 3;

[0062] Step S4: 10 mmol of intermediate 3, 50 mL of epichlorohydrin and 3.5 g of benzyltriethylammonium chloride were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture was stirred for reaction at a temperature of 95° C. and a stirring rate of 400 r / min for 8 h, and then 80 mL of a 25% sodium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 4;

[0063] Step S5: 100 g of intermediate 4 and 0.1 g of hydroquinone were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture was stirred at 55° C. and a stirring rate of 400 r / min for 15 min. Then, 0.9 g of benzyltriethylammonium chloride was added and the stirring reaction was continued for 10 min. Then, 70 g of acrylic acid was added dropwise while stirring, and the dropping rate was controlled to 2 drops / s. After the addition was completed, the mixture was heated to 110° C. and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature to obtain a high temperature resistant modified vinyl ester resin.

[0064] Step S6: adding 2 g of alkali-free glass fiber with a length of 3 mm and a diameter of 20 μm and 25 mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, introducing nitrogen protection, stirring the reaction for 10 min at a temperature of 30° C. and a stirring rate of 400 r / min, then heating to reflux and continuing to stir the reaction for 8 h, cooling the reaction product to room temperature after the reaction is completed, and then vacuum filtering, washing the filter cake with distilled water 5 times, and then placing it in a vacuum drying oven, and drying it at a temperature of 65° C. for 3 h to obtain washed glass fiber;

[0065] Step S7: 10 g of washed glass fiber, 0.09 g of hexadecyltrimethylammonium bromide, 35 mL of deionized water and 110 mL of anhydrous ethanol were added to a three-necked flask equipped with a thermometer, a stirrer and a reflux condenser, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, then 15 g of silane coupling agent KH-570 was added and the temperature was raised to reflux and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filter cake was washed with distilled water 5 times, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain modified glass fiber;

[0066] Step S8: weighing 120 parts of high temperature resistant modified vinyl ester resin, 24 parts of modified glass fiber, 55 parts of diluent, 1.9 parts of accelerator and 1.5 parts of initiator according to weight parts for standby use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate;

[0067] Step S9: Add the high temperature resistant modified vinyl ester resin, modified glass fiber and diluent into a mixer, stir and mix for 50 minutes at a temperature of 50°C and a stirring rate of 400 r / min, then add the accelerator and initiator and continue to stir and mix for 8 minutes, then pour into a mold, and then place in an oven, cure at a temperature of 75°C for 2.5 hours, and then heat to 100°C and cure for 1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0068] Comparative Example 1:

[0069] This comparative example is a method for preparing glass fiber reinforced plastic based on vinyl ester resin, comprising the following steps:

[0070] Step S1: 100 g of epoxy resin E-44 and 0.1 g of hydroquinone are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction at a temperature of 55° C. and a stirring rate of 400 r / min for 15 min, and then 0.9 g of benzyltriethylammonium chloride is added and the stirring reaction is continued for 10 min, and then 70 g of acrylic acid is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the addition is completed, the mixture is heated to 110° C. and the stirring reaction is continued for 3 h. After the reaction is completed, the reaction product is cooled to room temperature to obtain a vinyl ester resin;

[0071] Step S2: 120 parts of vinyl ester resin, 24 parts of alkali-free glass fiber, 55 parts of diluent, 1.9 parts of accelerator and 1.5 parts of initiator are weighed in parts by weight for later use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate;

[0072] Step S3: Add vinyl ester resin, alkali-free glass fiber and diluent into a mixer, stir and mix for 50 minutes at a temperature of 50°C and a stirring rate of 400 r / min, then add accelerator and initiator and continue to stir and mix for 8 minutes, then pour into a mold, and then place in an oven, cure at a temperature of 75°C for 2.5 hours, and then heat to 100°C and cure for 1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0073] Comparative Example 2:

[0074] This comparative example is a method for preparing glass fiber reinforced plastic based on vinyl ester resin, comprising the following steps:

[0075] Step S1: 10 mmol of melamine, 37 mmol of 3,5-dimethoxybenzaldehyde and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min, and then the mixture was heated to reflux and continued to be stirred for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed with distilled water for 5 times, and then placed in a vacuum drying oven and dried at a temperature of 85° C. for 5 h to obtain an intermediate 1;

[0076] Step S2: 10 mmol of intermediate 1, 35 mmol of DOPO and 100 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, and nitrogen protection was introduced. The mixture was stirred at 30° C. and a stirring rate of 400 r / min for 10 min, and then the temperature was raised to reflux and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;

[0077] Step S3: 10 mmol of intermediate 2 and 120 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a constant pressure dropping funnel, and nitrogen protection was introduced. The mixture was stirred for 30 min at a temperature of 0°C and a stirring rate of 400 r / min. Then, 55 mL of a boron tribromide solution formed by dissolving boron tribromide in dichloromethane at a ratio of 10 mmol:5 mL was added dropwise while stirring. The dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 30°C and the stirring reaction was continued for 15 h. After the reaction was completed, the reaction product was added to ice water, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 65°C for 5 h to obtain intermediate 3;

[0078] Step S4: 10 mmol of intermediate 3, 50 mL of epichlorohydrin and 3.5 g of benzyltriethylammonium chloride were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture was stirred for reaction at a temperature of 95° C. and a stirring rate of 400 r / min for 8 h, and then 80 mL of a 25% sodium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 4;

[0079] Step S5: 100 g of intermediate 4 and 0.1 g of hydroquinone were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture was stirred at 55° C. and a stirring rate of 400 r / min for 15 min. Then, 0.9 g of benzyltriethylammonium chloride was added and the stirring reaction was continued for 10 min. Then, 70 g of acrylic acid was added dropwise while stirring, and the dropping rate was controlled to 2 drops / s. After the addition was completed, the mixture was heated to 110° C. and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature to obtain a high temperature resistant modified vinyl ester resin.

[0080] Step S6: weighing 120 parts of high temperature resistant modified vinyl ester resin, 24 parts of alkali-free glass fiber, 55 parts of diluent, 1.9 parts of accelerator and 1.5 parts of initiator according to weight parts for later use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate;

[0081] Step S7: Add the high temperature resistant modified vinyl ester resin, alkali-free glass fiber and diluent into a mixer, stir and mix for 50 minutes at a temperature of 50°C and a stirring rate of 400 r / min, then add the accelerator and initiator and continue to stir and mix for 8 minutes, then pour into a mold, and then place in an oven, cure at a temperature of 75°C for 2.5 hours, and then heat to 100°C and cure for 1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0082] Comparative Example 3:

[0083] This comparative example is a method for preparing glass fiber reinforced plastic based on vinyl ester resin, comprising the following steps:

[0084] Step S1: 100 g of epoxy resin E-44 and 0.1 g of hydroquinone are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction at a temperature of 55° C. and a stirring rate of 400 r / min for 15 min, and then 0.9 g of benzyltriethylammonium chloride is added and the stirring reaction is continued for 10 min, and then 70 g of acrylic acid is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the addition is completed, the mixture is heated to 110° C. and the stirring reaction is continued for 3 h. After the reaction is completed, the reaction product is cooled to room temperature to obtain a vinyl ester resin;

[0085] Step S2: 2 g of alkali-free glass fiber with a length of 3 mm and a diameter of 20 μm and 25 mL of anhydrous acetone are added to a three-necked flask equipped with a stirrer, a thermometer, a nitrogen gas guide tube and a reflux condenser, and nitrogen protection is introduced. The mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 10 min, and then the temperature is raised to reflux and the stirring reaction is continued for 8 h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed with distilled water for 5 times, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain washed glass fiber;

[0086] Step S3: 10 g of washed glass fiber, 0.09 g of hexadecyltrimethylammonium bromide, 35 mL of deionized water and 110 mL of anhydrous ethanol were added to a three-necked flask equipped with a thermometer, a stirrer and a reflux condenser, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, then 15 g of silane coupling agent KH-570 was added and the temperature was raised to reflux and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filter cake was washed with distilled water 5 times, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain modified glass fiber;

[0087] Step S4: weighing 120 parts of vinyl ester resin, 24 parts of modified glass fiber, 55 parts of diluent, 1.9 parts of accelerator and 1.5 parts of initiator according to weight parts for standby use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate;

[0088] Step S5: Add vinyl ester resin, modified glass fiber and diluent into a mixer, stir and mix for 50 minutes at a temperature of 50°C and a stirring rate of 400 r / min, then add accelerator and initiator and continue to stir and mix for 8 minutes, then pour into a mold, and then place in an oven, cure at a temperature of 75°C for 2.5 hours, and then heat to 100°C and cure for 1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.

[0089] The glass fiber reinforced plastics based on vinyl ester resin of Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the test results are as follows:

[0090] sample Tensile strength, MPa Bending strength, MPa Heat deformation temperature, °C Limiting oxygen index, % Example 1 162 240 248 40 Example 2 169 252 251 43 Example 3 175 261 253 47 Comparative Example 1 108 177 183 31 Comparative Example 2 149 229 244 45 Comparative Example 3 134 213 196 33

[0091] Referring to the data in the above table, based on the comparison between Examples 1-3 and Comparative Examples 1-3, it can be known that the glass fiber reinforced plastic based on vinyl ester resin in the present invention has excellent mechanical strength and high temperature resistance and flame retardancy.

[0092] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0093] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. Glass fiber reinforced plastic based on vinyl ester resin, characterized in that It comprises the following components in parts by weight: 80-120 parts of high temperature resistant modified vinyl ester resin, 6-24 parts of modified glass fiber, 35-55 parts of diluent, 1.3-1.9 parts of accelerator and 0.9-1.5 parts of initiator; Wherein, the high temperature resistant modified vinyl ester resin is prepared by the following steps: Step A1: stirring melamine, 3,5-dimethoxybenzaldehyde and anhydrous ethanol for reaction, cooling the reaction product after the reaction is completed, and then vacuum filtering, washing and drying the filter cake to obtain intermediate 1; Step A2: The intermediate 1, DOPO and N,N-dimethylformamide are stirred for reaction. After the reaction is completed, the reaction product is cooled, then vacuum filtered, and the filtrate is rotary evaporated to obtain the intermediate 2; Step A3: Stir the intermediate 2 and dichloromethane for reaction, then add the boron tribromide solution dropwise while stirring, continue stirring for reaction after the addition is complete, add the reaction product into ice water after the reaction is complete, then vacuum filter, and dry the filter cake to obtain the intermediate 3; Step A4: stirring the intermediate 3, epichlorohydrin and benzyltriethylammonium chloride for reaction, then adding sodium hydroxide solution dropwise while stirring, and continuing to stir the reaction after the addition is complete. After the reaction is complete, the reaction product is cooled and then rotary evaporated to obtain the intermediate 4; Step A5: Stir the intermediate 4 and hydroquinone for reaction, then add benzyltriethylammonium chloride and continue to stir the reaction, then add acrylic acid dropwise while stirring, continue to stir the reaction after the dropwise addition is completed, and cool the reaction product after the reaction is completed to obtain a high temperature resistant modified vinyl ester resin; The modified glass fiber is prepared by the following steps: Step B1: stirring the glass fiber and anhydrous acetone to react, cooling the reaction product after the reaction is completed, and then vacuum filtering, washing and drying the filter cake to obtain washed glass fiber; Step B2: Stir the washed glass fiber, hexadecyltrimethylammonium bromide, deionized water and anhydrous ethanol for reaction, then add the silane coupling agent KH-570 and continue stirring the reaction. After the reaction is completed, cool the reaction product, then vacuum filter, wash and dry the filter cake to obtain modified glass fiber.

2. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The usage ratio of melamine, 3,5-dimethoxybenzaldehyde and anhydrous ethanol in step A1 is 10mmol:33-37mmol:50-60mL.

3. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The usage ratio of the intermediate 1, DOPO and N,N-dimethylformamide in step A2 is 10 mmol: 30-35 mmol: 90-100 mL.

4. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The dosage ratio of the intermediate 2, dichloromethane and boron tribromide solution in step A3 is 10 mmol: 100-120 mL: 50-55 mL; the boron tribromide solution in step A3 is a solution formed by dissolving boron tribromide in dichloromethane at a ratio of 8-10 mmol: 5 mL.

5. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The usage ratio of the intermediate 3, epichlorohydrin, benzyltriethylammonium chloride and sodium hydroxide solution in step A4 is 10mmol:40-50mL:2.5-3.5g:60-80mL; the mass fraction of the sodium hydroxide solution in step A4 is 20-25%.

6. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The usage ratio of the intermediate 4, hydroquinone, benzyltriethylammonium chloride and acrylic acid in step A5 is 100g: 0.05-0.1g: 0.3-0.9g: 40-70g.

7. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The usage ratio of the glass fiber and anhydrous acetone in step B1 is 2g:20-25mL; the glass fiber in step B1 is an alkali-free glass fiber with a length of 3mm and a diameter of 20μm.

8. The glass fiber reinforced plastic based on vinyl ester resin according to claim 1, characterized in that The amount ratio of the washed glass fiber, hexadecyltrimethylammonium bromide, deionized water, anhydrous ethanol and silane coupling agent KH-570 in step B2 is 10g: 0.05-0.09g: 25-35mL: 100-110mL: 7.5-15g.

9. A method for preparing a glass fiber reinforced plastic based on vinyl ester resin according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Weigh 80-120 parts of high temperature resistant modified vinyl ester resin, 6-24 parts of modified glass fiber, 35-55 parts of diluent, 1.3-1.9 parts of accelerator and 0.9-1.5 parts of initiator according to weight parts for use; the diluent is styrene, the accelerator is cobalt isooctanoate, and the initiator is tert-butyl peroxy 2-ethylhexanoate; Step 2: Add the high temperature resistant modified vinyl ester resin, modified glass fiber and diluent into a mixer, stir and mix for 30-50 minutes at a temperature of 45-50°C and a stirring rate of 300-400r / min, then add the accelerator and initiator and continue to stir and mix for 5-8 minutes, then pour into a mold, and then place in an oven, and cure at a temperature of 70-75°C for 2-2.5 hours, and then heat to 95-100°C and cure for 0.5-1 hour to obtain a glass fiber reinforced plastic based on vinyl ester resin.